NEW BLENDED CEMENTS
PRINCIPAL DEVELOPMENT GOALS
 REDUCING CARBON (GHG) EMISSION THROUGH
CLINKER SUBSTITUTION
 REDUCING ENERGY CONSUMPTION
 INCREASED PRODUCTION CAPACITY
REDUCING SOLID WASTE
 MAINTAINING QUALITY : STRENGTH & DURABILITY
NEW BLENDED CEMENTS
IS 456 – 2000 PROVISIONS
ADMIXTURES PERMITTED BY INDIAN STANDARD CODE
FOR PLAIN AND REINFORCED CONCRETE i.e. IS 456 – 2000
 FLY ASH (15-35% )
 BLAST FURNACE SLAG OR GGBS (25-70%)
 SILICA FUME (3-10%)*
 RICE HUSK ASH (25-30%)*
 METAKAOLIN (10-25%)*
* Recommended as per common practice
NEW BLENDED CEMENTS
 PORTLAND LIMESTONE CEMENT (PLC)
 PORTLAND HIGH VOLUME FLY ASH CEMENT (PHFC)
PORTLAND LIMESTONE CEMENT
PLC
NEW BLENDED CEMENTS
PORTLAND LIMESTONE CEMENT (PLC)
INDIAN & INTERNATIONAL STANDARDS
 INDIAN STANDARD IS 269 - 2013: PERMITS ADDITION OF LIMESTONE UPTO 5%,
AS PERFORMANCE IMPROVER, IN OPC
 EUROPEAN STANDARD EN 197-1 (2000):
 5% LS ADDITION PERMITTED IN ALL 27 APPROVED TYPES, AS MINOR
ADDITIONAL CONSTITUENT (MAC)
 OUT OF THAT, 4 ARE PORTLAND LIMESTONE CEMENT, PERMITTING HIGHER
ADDITIONS OF LS, IN ADDITION TO 5% MAC AS ABOVE
 CEM II/A-L & CEM II/A-LL: 6 TO 20% & CEM II/B-L & CEM II/B-LL: 21-35%
 US STANDARDS:
 ASTM C150: 5% LS ADDITION PERMITTED IN TYPES I TO V
 ASTM C595 & AASHTO M240: 5-15% LS ADDITION PERMITTED IN TYPE IL & IT
CANADIAN STANDARD CSA A3001:
 5% LS ADDITION PERMITTED IN PORTLAND CEMENT
 6 - 15% LS ADDITION PERMITTED PORTLAND LIMESTONE CEMENT
NEW BLENDED CEMENTS
PORTLAND LIMESTONE CEMENT (PLC)
SIGNIFICANCE OF 15% LIMIT
Matschei et al. 2007
NEW BLENDED CEMENTS
PORTLAND LIMESTONE CEMENT (PLC)
HOW LIMESTONE WORKS
PARTICLE PACKING – IMPROVED PARTICLE SIZE DISTRIBUTION
NEW BLENDED CEMENTS
PORTLAND LIMESTONE CEMENT (PLC)
HOW LIMESTONE WORKS
PROVIDES NUCLEATION SURFACES
FOR PRECIPITATION OF HYDRATED CEMENT
NEW BLENDED CEMENTS
PORTLAND LIMESTONE CEMENT (PLC)
HOW LIMESTONE WORKS
LS REACTS WITH ALUMINATES IN
CEMENT TO FORM CARBOALUMINATES
NEW BLENDED CEMENTS
PORTLAND LIMESTONE CEMENT (PLC)
LIMESTONE REQUIREMENTS: EN STANDARDS
 CALCIUM CARBONATE > 75%
 TOTAL ORGANIC CARBON (TOC): MAX 0.5%
 CLAY: MAX 1.2 g/100g
NEW BLENDED CEMENTS
PORTLAND LIMESTONE CEMENT (PLC)
PRODUCTION OF PLC
 METERED PROPORTION OF CRUSHED, DRIED LS FED TO FINISH GRINDING
MILL ALONG, WITH CLINKER & GYPSUM
 LS IS MORE EASILY GROUND THAN CLINKER (HARDER) & GETS
CONCENTRATED IN FINE PARTICLES
 OVERALL FINENESS MUST BE HIGHER, FOR EQUIVALENT PERF (.) TO HAVE
FINENESS OF THE CLINKER FRACTION TO BE SIMILAR TO OPC:
 PRODUCTION RATE IS SLOWED
 SOME ADDITIONAL GRINDING ENERGY REQUIRED BUT IS MORE THAN
OFFSET BY LOWER CLINKER CONTENT & RELATED KILN FUEL SAVINGS
 PARTICLE SIZE DISTRIBUTION IS ENHANCED
 HYDRATION IS ENHANCED BY BOTH PHYSICAL AND CHEMICAL INTERACTION
 SUSTAINABILITY BENEFITS SIGNIFICANT: REDUCED ASSOCIATED CARBON
EMISSIONS & EMBODIED ENERGY (LESS CLINKER)
NEW BLENDED CEMENTS
PORTLAND LIMESTONE CEMENT (PLC)
PRODUCTION PLC
INTER-GRINDING WITH CLINKER
GRINDING ENERGY CONSUMPTION DECREASES WITH LS REPLACEMENT
Opoczky, L., 1992
NEW BLENDED CEMENTS
PORTLAND LIMESTONE CEMENT (PLC)
FRESH CONCRETE WITH PLC
 WATER DEMAND & WORKABILITY RELATED TO PARTICLE SIZE
DISTRIBUTION OF LS IN RELATION TO CEMENT
 GENERALLY INCREASED WATER IS NEEDED TO MAINTAIN
CONSISTENCY OF CEMENT PASTES AS LS CONTENT INCREASES
FINE LS PARTICLES ENHANCE OVERALL PARTICLE PACKING OF
BINDER MATERIALS RESULTING IN LESS SPACE FOR WATER
BETWEEN SOLID GRAINS
DECREASING AVERAGE PARTICLE SIZE OF LS GIVES BETTER
EARLY-AGE RHEOLOGICAL PROPERTIES
NEW BLENDED CEMENTS
PORTLAND LIMESTONE CEMENT (PLC)
FRESH CONCRETE WITH PLC
REDUCED BLEEDING
Specific Surface Area m2/kg
Building Research
Establishment , 1993
NEW BLENDED CEMENTS
PORTLAND LIMESTONE CEMENT (PLC)
FRESH CONCRETE WITH PLC
HYDRATION
 AS LIMESTONE ACTS AS NUCLEATION
SITES FOR HYDRATION PRODUCTS ITS
INCLUSION INCREASES RATE OF HYDRATION
 LIMESTONE ADDITIONS GIVE EARLIER
PEAK FOR HEAT OF HYDRATION
NEW BLENDED CEMENTS
PORTLAND LIMESTONE CEMENT (PLC)
MECHANICAL PROPERTIES: CONCRETE WITH PLC
 LS UP TO 5% INCREASES EARLY-AGE STRENGTH DUE TO: IMPROVED PARTICLE
PACKING , INCREASED RATE OF CEMENT HYDRATION & EARLY PRODUCTION OF
CALCIUM CARBOALUMINATE (.) APPLIES TO BOTH INTER-GROUND & BLENDED PLC
 HIGHER REPLACEMENTS: LOSS OF STRENGTH DUE TO DILUTION MUST BE
COMPENSATED BY FINER GRINDING (.) VOGLIS ET AL (2005): SHOWED COMPARABLE
STRENGTHS FOR PC & PLC WITH 15% LS, WHEN PLC WAS GROUND TO 511 m2/kg
COMPARED WITH 303 m2/kg FOR PC
 TSIVILIS ET AL (1999): APPROPRIATE CHOICE OF CLINKER QUALITY, LS QUALITY, %
LS CONTENT & CEMENT FINENESS CAN LEAD TO PRODUCTION OF PLC WITH
DESIRED PROPERTIES, AT LEAST FOR CEMENTS WITH UP TO 15% LS
 TENSILE, FLEXURAL STRENGTH & MODULUS OF ELASTICITY: STANDARD
EQUATIONS APPLICABLE (.) SHRINKAGE SAME BUT CREEP INCREASES
NEW BLENDED CEMENTS
PORTLAND LIMESTONE CEMENT (PLC)
DURABILITY OF CONCRETE WITH PLC
CONCRETE PERMEABILITY
Matthews, J.D. 1994.
NEW BLENDED CEMENTS
PORTLAND LIMESTONE CEMENT (PLC)
DURABILITY OF CONCRETE WITH PLC
CHLORIDE DIFFUSION COEFFICIENT
Dhir, R.K., et.al. 2007.
NEW BLENDED CEMENTS
PORTLAND LIMESTONE CEMENT (PLC)
DURABILITY OF CONCRETE WITH PLC
CARBONATION
Dhir, R.K., et.al. 2007
NEW BLENDED CEMENTS
PORTLAND LIMESTONE CEMENT (PLC)
DURABILITY OF CONCRETE WITH PLC
CARBONATION
 IN REFERENCE TO HYDRATED PLC, STRENGTH OF PLC AFTER
ACCELERATED CARBONATION WAS 79% HIGHER AT 28 D, EVEN THOUGH
ULTIMATE LS CONTENT IN CARBONATED PLC WAS OVER 40%
 CALCIUM CARBONATES PRODUCED BY ACCELERATED CARBONATION
GETS IMBEDDED IN C-S-H, FORMING INTERMINGLED MICROSTRUCTURE
 HIGH CARBONATION REACTIVITY OF PLC ATTRIBUTED TO FINE PARTICLE
SIZE & EXISTENCE OF LS POWDER NUCLEI FOR CALCIUM CARBONATE
PRECIPITATION
 USE OF PLC IN ACCELERATED CARBONATION OF CONCRETE PRODUCTS
CAN SIGNIFICANTLY CONTRIBUTE TO A NET GAIN IN STRENGTH & CARBON
EMISSION REDUCTION
Ref: Shao Y., et. al. 2014
NEW BLENDED CEMENTS
PORTLAND LIMESTONE CEMENT (PLC)
DURABILITY OF CONCRETE WITH PLC
SULPHATE RESISTANCE
 STANDARDS DO NOT RECOMMEND USE OF PLC IN SULPHATE
ENVIRONMENT
 AT NORMAL TEMPERATURE, SULPHATE RESISTANCE OF PLC IS
SUBSTANTIALLY IMPROVED WHEN 30-50% SLAG IS ADDED & LS
REPLACEMENT OF 5-15% ARE ALLOWABLE
 SIMILARLY AT 5 C ALSO, SULPHATE RESISTANCE IS SUBSTANTIALLY
IMPROVED WITH THE ADDITION OF SLAG
Ref: Ramezanianpour A. M., 2012
NEW BLENDED CEMENTS
PORTLAND LIMESTONE CEMENT (PLC)
DURABILITY OF CONCRETE WITH PLC
OTHER DURABILITY PARAMETERS
 SALT SCALING & FREEZE-THAW: LIMITED DATA AVAILABLE FOR AIR-
ENTRAINED CONCRETE SHOW THAT FREEZE-THAW & SALT SCALING
RESISTANCE OF PLC CONCRETE IS COMPARABLE TO THAT OF EQUIVALENT
PC CONCRETE
 ABRASION RESISTANCE: CONCRETES OF IDENTICAL 28-DAY STRENGTH
HAVE SIMILAR ABRASION RESISTANCE, IRRESPECTIVE OF LS CONTENT OF
CEMENT
NEW BLENDED CEMENTS
PORTLAND LIMESTONE CEMENT (PLC)
SUMMARY
 LS CEMENTS HAVE BEEN USED IN MANY COUNTRIES SINCE THE 1960’S & EU CEM
II/A 6 TO 20% LIMESTONE CEMENTS ARE THE LARGEST SINGLE TYPE OF CEMENT
CURRENTLY PRODUCED IN EUROPEAN COUNTRIES
 LS FINENESS & PARTICLE SIZE DISTRIBUTION ARE KEY PARAMETRS
ADVANTAGES:
 PLC RESULTS IN REDUCED GHG EMISSIONS
 WHEN PROPERLY OPTIMISED, PLC CONCRETE HAS FRESH PROPERTIES,
BLEEDING & STRENGTH SIMILAR TO OPC CONCRETE
REDUCED PERMEABILITY
 SIMILAR CHLORIDE DURABILITY UP TO 15% REPLACEMENT
 SIMILAR CARBONATION RATE UP TO 15% REPLACEMENT, AT LOW W/C RATIO
 SUBSTANTIALLY IMPROVED SULPHATE RESISTANCE, WHEN PLC UP TO 15% LS, IS
BLENDED WITH SLAG WITH 50% REPLACEMENT
DISADVANTAGE:
 PERFORMANCE IS AFFECTED BY (A) QUALITY OF LS, (B) WHETHER INTERGROUND
OR BLENDED & (C) PARTICLE SIZE DISTRIBUTION
PORTLAND HIGH VOLUME FLY ASH CEMENT
PHFC
NEW BLENDED CEMENTS
PORTLAND HIGH VOLUME FLY ASH CEMENT (PHFC)
PHFC REFERS TO BLENDED CEMENT PRODUCED IN CEMENT PLANT,
WITH FA REPLACEMENT CEMENT >55%
AT PRESENT HIGH VOLUMES OF FA (>55%) ARE ADDED AS REPLACEMENT
OF CEMENT, AT RMC PLANTS, TO PRODUCE HIGH VOLUME FLY ASH
CONCRETE (HVFAC) (.) IT NECESSITATES ADDITIONAL STORAGE SILOS &
QUALITY CONTROL AT JOB SITE
PHFC IS ONE OPTION, INCREASING AMOUNT OF FA THAT CAN REPLACE
PORTLAND CEMENT (PC) FROM <20% IN CONVENTIONAL MIXES UP TO AS
HIGH AS 55%
PHFC CAN BE PRODUCED EITHER BY INTER-GRINDING FA WITH PC
CLINKER & GYPSUM OR BY BLENDING DRY FA WITH PC (.) SOMETIMES DRY
SUPER PLASTICISER IS ALSO INTERGROUND (.) PRODUCTION OF PHFC
USING INTER-GRINDING METHOD APPEARS MOST COST-EFFECTIVE &
PRACTICAL
REQUIRED TO SATISFY MINIMUM STRENGTH AS PER ASTM C1157, OF 10 &
17 MPa AT 3 & 7 DAYS RESPECTIVELY
NEW BLENDED CEMENTS
PORTLAND HIGH VOLUME FLY ASH CEMENT (PHFC)
WHY INTER-GRINDING
EFFECT OF GRINDING ON FA PROPERTIES
 SPECIFIC GRAVITY: INCREASES DUE TO CRUSHING OF PLEROSHERES
AND CENOSHERES AND CONTUES FOR CERTAIN TIME PERIOD OF
GRINDING
 SPECIFIC SURFACE: INCREASES WITH GRINDING TIME, BUT AT THE
EXPENSE OF GRINDING ENERGY
 MORPHOLOGY: OPTIMUM GRINDING PERIOD DOES NOT AFFECT
SPHERICAL SHAPE OF FA PARTICLES SIGNIFICANTLY
 WATER REQUIREMENT OF MORTAR: DECREASES UP TO CERTAIN TIME
PERIOD & LATER INCREASES (.) RELATED TO SPHERICAL SHAPE
 POZZOLANIC ACTIVITY: INCREASES AT RAPID RATE UP TO CERTAIN TIME
PERIOD, LATER RATE DECREASES
 THESE ASPECTS SHOW PHFC SHOULD BE PREFERABLY PRODUCED BY
INTER-GRINDING & GRINDING PERIOD SHOULD BE OPTIMISED.
NEW BLENDED CEMENTS
PORTLAND HIGH VOLUME FLY ASH CEMENT (PHFC)
GRINDING SUPERPLASTICISER WITH CLINKER & GYPSUM
WHEN NAPHTHALINE BASED SP WAS VARIED FROM 0-0.9% (MASS OF
CLINKER+GYPSUM):
 GRINDING TIME: SP ACTED AS GRINDING AID & GRINDING TIME REDUCED
TO OBTAIN REQUIRED BLAINE FINENESS
 WATER REQUIREMENT & COMPRESSIVE STRENGTH: SP ADDITION
DURING GRINDING OR SEPARATELY AT THE MIXER PRODUCED SAME
EFFECT
 BLAINE: FIXED ON THE BASIS OF FA, BY CARRYING OUT TRIALS
 BETTER TO ADD SP AT THE GRINDING STAGE
 ADDITION OF SP ALSO ELIMINATES COMPATIBILITY ISSUES AT
CONCRETING STAGE
 PREDETERMINED QUANTITY OF SP MAY BE ADDED TO OBTAIN REQUIRED
CONCRETE SLUMP
NEW BLENDED CEMENTS
PORTLAND HIGH VOLUME FLY ASH CEMENT (PHFC)
CONCRETE WITH PHFC
RESULTS OF LABORATORY TRIALS ON PHFC WITH 55% FA*
 FRESH CONCRETE: CONCRETE WITH PHFC REQUIRED MORE SP & AEA,
AS INTER-GRINDING INCREASED FINENESS
 COMPRESSIVE STRENGTH: IRRESPECTIVE OF SOURCE & TYPE OF FA,
CONCRETE WITH PHFC DEVELOPED BETTER STRENGTH COMPARED TO
THAT PREPARED BY SEPARATE ADDITION OF CEMENT & UN-GROUND FA AT
MIXER
 CHLORIDE RESISTANCE: INTER-GRINDING IMPROVED CHLORIDE
RESISTANCE OF CONCRETE
*Ref: Electric Power Research Institute (EPRI), USA, 2001
NEW BLENDED CEMENTS
PORTLAND HIGH VOLUME FLY ASH CEMENT (PHFC)
SUMMARY
PHFC IS FACTORY MADE WITH FA REPLACING CEMENT AT 55%
ADDING SP TO CLINKER AT FINISH GRINDING STAGE HELP REDUCE
GRINDING ENERGY & ALSO SOLVES COMPATIBILITY ISSUES AT
CONCRETING STAGE
INTER-GRINDING FA WITH GROUND CEMENT FOR FIXED TIME PERIOD
IMPARTS BETTER CONCRETE PROPERTIES
PHFC HAS VERY GOOD RESISTANCE TOWARDS CHLORIDE PENETRATION
NEW BLENDED CEMENTS
 NO CEMENT OR ADMIXTURE CAN OFFSET LOW QUALITY CONCRETE
 DURABLE CONCRETE DEPENDS ON:
 APPROPRIATE MIXTURE PROPORTIONS
 LOWER w/c RATIO
 PROPER PLACEMENT
 CURING
 MAINTENANCE
 WHEN GOOD PRACTICES ARE FOLLOWED, CONCRETE WILL ATTAIN ITS
EXPECTED SERVICE LIFE
JOIN MY NETWORK
YOU ARE WELCOME TO JOIN ME
 FACEBOOK: Jayant D Bapat
 TWITTER: @cemcretecon & @drjdbapat
 LINKEDIN: Dr J. D. Bapat
(email: jdbapat@yahoo.co.in)
 EMAIL_1: consult@drjdbapat.com
 EMAIL_2: consult.bapat@yahoo.com
 URL: http://www.drjdbapat.com
NEW BLENDED CEMENTS
Thanks!!!

More Related Content

What's hot

What's hot (20)

Superplasticizers
SuperplasticizersSuperplasticizers
Superplasticizers
 
Cement chemical
Cement  chemicalCement  chemical
Cement chemical
 
STRENGTH PROPERTIES OF CONCRETE BY USING RED MUD AS A REPLACEMENT OF CEMENT W...
STRENGTH PROPERTIES OF CONCRETE BY USING RED MUD AS A REPLACEMENT OF CEMENT W...STRENGTH PROPERTIES OF CONCRETE BY USING RED MUD AS A REPLACEMENT OF CEMENT W...
STRENGTH PROPERTIES OF CONCRETE BY USING RED MUD AS A REPLACEMENT OF CEMENT W...
 
Presentation on pervios concrete
Presentation on pervios concretePresentation on pervios concrete
Presentation on pervios concrete
 
Geopolymer concrete ppt
Geopolymer concrete pptGeopolymer concrete ppt
Geopolymer concrete ppt
 
light weight concrete
light weight concretelight weight concrete
light weight concrete
 
Geopolymer concrete
Geopolymer concreteGeopolymer concrete
Geopolymer concrete
 
Concrete Admixtures
 Concrete Admixtures Concrete Admixtures
Concrete Admixtures
 
Geopolymer concrete
Geopolymer concreteGeopolymer concrete
Geopolymer concrete
 
Fibre reinforced concrete
Fibre reinforced concreteFibre reinforced concrete
Fibre reinforced concrete
 
No fines concrete
No fines concreteNo fines concrete
No fines concrete
 
Foam Concrete/Light Weight Concrete.
Foam Concrete/Light Weight Concrete.Foam Concrete/Light Weight Concrete.
Foam Concrete/Light Weight Concrete.
 
History of admixtures
History of admixturesHistory of admixtures
History of admixtures
 
Silica fume
Silica fumeSilica fume
Silica fume
 
Flyash
FlyashFlyash
Flyash
 
Silica fume
Silica fumeSilica fume
Silica fume
 
High Performance Concrete
High Performance ConcreteHigh Performance Concrete
High Performance Concrete
 
What is Portland Slag Cement ?
What is  Portland Slag Cement ?What is  Portland Slag Cement ?
What is Portland Slag Cement ?
 
cement ppt
cement pptcement ppt
cement ppt
 
Special Concrete - Concrete Technology
Special Concrete - Concrete TechnologySpecial Concrete - Concrete Technology
Special Concrete - Concrete Technology
 

Similar to NEW BLENDED CEMENTS

FLY ASH MATERIALS
FLY ASH MATERIALS FLY ASH MATERIALS
FLY ASH MATERIALS
bholenath999
 
glo-sika-additives-calcined-clay-cements.pdf
glo-sika-additives-calcined-clay-cements.pdfglo-sika-additives-calcined-clay-cements.pdf
glo-sika-additives-calcined-clay-cements.pdf
Luan Bici
 

Similar to NEW BLENDED CEMENTS (20)

ppt meghaaaaaa (1)al.pptx
ppt meghaaaaaa (1)al.pptxppt meghaaaaaa (1)al.pptx
ppt meghaaaaaa (1)al.pptx
 
Construction Materials
Construction Materials Construction Materials
Construction Materials
 
Bapat low_carbon_tech_cbi india 2015
Bapat low_carbon_tech_cbi india 2015Bapat low_carbon_tech_cbi india 2015
Bapat low_carbon_tech_cbi india 2015
 
IBAUSIL_FAST SET GGBS BINDER _Presentatie.pptx
IBAUSIL_FAST SET GGBS BINDER _Presentatie.pptxIBAUSIL_FAST SET GGBS BINDER _Presentatie.pptx
IBAUSIL_FAST SET GGBS BINDER _Presentatie.pptx
 
FLY ASH MATERIALS
FLY ASH MATERIALS FLY ASH MATERIALS
FLY ASH MATERIALS
 
geopolymerconcrete-Introduction and .pptx
geopolymerconcrete-Introduction and .pptxgeopolymerconcrete-Introduction and .pptx
geopolymerconcrete-Introduction and .pptx
 
CALUMEX Q_cem_Presentatie_Final_Final.pdf
CALUMEX Q_cem_Presentatie_Final_Final.pdfCALUMEX Q_cem_Presentatie_Final_Final.pdf
CALUMEX Q_cem_Presentatie_Final_Final.pdf
 
ppt meghaaaaaa (1).pdf
ppt meghaaaaaa (1).pdfppt meghaaaaaa (1).pdf
ppt meghaaaaaa (1).pdf
 
High volume fly ash concrete
High volume fly ash concreteHigh volume fly ash concrete
High volume fly ash concrete
 
Cement
CementCement
Cement
 
Coal Ashes In Geo-technical Engineering Practice-Beneficial Aspects
Coal Ashes In Geo-technical Engineering Practice-Beneficial AspectsCoal Ashes In Geo-technical Engineering Practice-Beneficial Aspects
Coal Ashes In Geo-technical Engineering Practice-Beneficial Aspects
 
Fly ash concrete
Fly ash concreteFly ash concrete
Fly ash concrete
 
Effect of Silica Fume on High Strength High Volume Fly Ash Concrete
Effect of Silica Fume on High Strength High Volume Fly Ash ConcreteEffect of Silica Fume on High Strength High Volume Fly Ash Concrete
Effect of Silica Fume on High Strength High Volume Fly Ash Concrete
 
Dr. Jayant D. Bapat - Durable and Sustainable Concrete with Mineral Admixture...
Dr. Jayant D. Bapat - Durable and Sustainable Concrete with Mineral Admixture...Dr. Jayant D. Bapat - Durable and Sustainable Concrete with Mineral Admixture...
Dr. Jayant D. Bapat - Durable and Sustainable Concrete with Mineral Admixture...
 
glo-sika-additives-calcined-clay-cements.pdf
glo-sika-additives-calcined-clay-cements.pdfglo-sika-additives-calcined-clay-cements.pdf
glo-sika-additives-calcined-clay-cements.pdf
 
Rpc seminar
Rpc seminarRpc seminar
Rpc seminar
 
COLD MIX ASPHALT.pptx
COLD MIX ASPHALT.pptxCOLD MIX ASPHALT.pptx
COLD MIX ASPHALT.pptx
 
Cement and Concrete: Promise of Fly Ash
Cement and Concrete: Promise of Fly AshCement and Concrete: Promise of Fly Ash
Cement and Concrete: Promise of Fly Ash
 
Use of marble dust
Use of marble dustUse of marble dust
Use of marble dust
 
Potassium formate brine with Micromax
Potassium formate brine with MicromaxPotassium formate brine with Micromax
Potassium formate brine with Micromax
 

More from Dr J.D. Bapat

More from Dr J.D. Bapat (18)

Dr j d bapat making of_sustainable_cement_and_concrete
Dr j d bapat making of_sustainable_cement_and_concreteDr j d bapat making of_sustainable_cement_and_concrete
Dr j d bapat making of_sustainable_cement_and_concrete
 
Cement based building_materials_icr_aug2020
Cement based building_materials_icr_aug2020Cement based building_materials_icr_aug2020
Cement based building_materials_icr_aug2020
 
FEEDBACK ON Dr J D BAPAT'S TRAINING COURSE ON CONCRETE AT L&T
FEEDBACK ON Dr J D BAPAT'S TRAINING COURSE ON CONCRETE AT L&TFEEDBACK ON Dr J D BAPAT'S TRAINING COURSE ON CONCRETE AT L&T
FEEDBACK ON Dr J D BAPAT'S TRAINING COURSE ON CONCRETE AT L&T
 
Orissa High Court Arbitration Centre Registration
Orissa High Court Arbitration Centre RegistrationOrissa High Court Arbitration Centre Registration
Orissa High Court Arbitration Centre Registration
 
Dr j d bapat_arbitrator_punjab_haryana_high_court_registration
Dr j d bapat_arbitrator_punjab_haryana_high_court_registrationDr j d bapat_arbitrator_punjab_haryana_high_court_registration
Dr j d bapat_arbitrator_punjab_haryana_high_court_registration
 
Dr J D Bapat_Academic_Adviser_Expertise_Summary
Dr J D Bapat_Academic_Adviser_Expertise_SummaryDr J D Bapat_Academic_Adviser_Expertise_Summary
Dr J D Bapat_Academic_Adviser_Expertise_Summary
 
J d bapat_durability_of_concrete
J d bapat_durability_of_concreteJ d bapat_durability_of_concrete
J d bapat_durability_of_concrete
 
Academic Adviser Engineering Education
Academic Adviser Engineering EducationAcademic Adviser Engineering Education
Academic Adviser Engineering Education
 
Dr J D Bapat_ICA Empanelment and Fellowship (FICA)
Dr J D Bapat_ICA Empanelment and Fellowship (FICA) Dr J D Bapat_ICA Empanelment and Fellowship (FICA)
Dr J D Bapat_ICA Empanelment and Fellowship (FICA)
 
Dr J D Bapat: Indian Council of Arbitration: Life Membership
Dr J D Bapat: Indian Council of Arbitration: Life MembershipDr J D Bapat: Indian Council of Arbitration: Life Membership
Dr J D Bapat: Indian Council of Arbitration: Life Membership
 
Ambuja cement panel_durability_28_may2016
Ambuja cement panel_durability_28_may2016Ambuja cement panel_durability_28_may2016
Ambuja cement panel_durability_28_may2016
 
Slide show non_destructive_testing
Slide show non_destructive_testingSlide show non_destructive_testing
Slide show non_destructive_testing
 
Slide show durability_of_concrete
Slide show durability_of_concreteSlide show durability_of_concrete
Slide show durability_of_concrete
 
Slide show concrete_with_blended_cement
Slide show concrete_with_blended_cementSlide show concrete_with_blended_cement
Slide show concrete_with_blended_cement
 
CEMENT TECHNOLOGY: FUTURISTIC TRENDS
CEMENT TECHNOLOGY: FUTURISTIC TRENDSCEMENT TECHNOLOGY: FUTURISTIC TRENDS
CEMENT TECHNOLOGY: FUTURISTIC TRENDS
 
ICI-JDB Certificate of Training in Durability of Concrete (C-TDC)
ICI-JDB Certificate of Training in Durability of Concrete (C-TDC) ICI-JDB Certificate of Training in Durability of Concrete (C-TDC)
ICI-JDB Certificate of Training in Durability of Concrete (C-TDC)
 
DURABLE CONCRETE WITH MINERAL ADMIXTURES: TRAINING COURSE IN MALAYSIA: BY Dr ...
DURABLE CONCRETE WITH MINERAL ADMIXTURES: TRAINING COURSE IN MALAYSIA: BY Dr ...DURABLE CONCRETE WITH MINERAL ADMIXTURES: TRAINING COURSE IN MALAYSIA: BY Dr ...
DURABLE CONCRETE WITH MINERAL ADMIXTURES: TRAINING COURSE IN MALAYSIA: BY Dr ...
 
Quality management for_engineering_institutions
Quality management for_engineering_institutionsQuality management for_engineering_institutions
Quality management for_engineering_institutions
 

Recently uploaded

1893-part-1-2016 for Earthquake load design
1893-part-1-2016 for Earthquake load design1893-part-1-2016 for Earthquake load design
1893-part-1-2016 for Earthquake load design
AshishSingh1301
 
Maher Othman Interior Design Portfolio..
Maher Othman Interior Design Portfolio..Maher Othman Interior Design Portfolio..
Maher Othman Interior Design Portfolio..
MaherOthman7
 
ALCOHOL PRODUCTION- Beer Brewing Process.pdf
ALCOHOL PRODUCTION- Beer Brewing Process.pdfALCOHOL PRODUCTION- Beer Brewing Process.pdf
ALCOHOL PRODUCTION- Beer Brewing Process.pdf
Madan Karki
 

Recently uploaded (20)

analog-vs-digital-communication (concept of analog and digital).pptx
analog-vs-digital-communication (concept of analog and digital).pptxanalog-vs-digital-communication (concept of analog and digital).pptx
analog-vs-digital-communication (concept of analog and digital).pptx
 
Passive Air Cooling System and Solar Water Heater.ppt
Passive Air Cooling System and Solar Water Heater.pptPassive Air Cooling System and Solar Water Heater.ppt
Passive Air Cooling System and Solar Water Heater.ppt
 
1893-part-1-2016 for Earthquake load design
1893-part-1-2016 for Earthquake load design1893-part-1-2016 for Earthquake load design
1893-part-1-2016 for Earthquake load design
 
Fuzzy logic method-based stress detector with blood pressure and body tempera...
Fuzzy logic method-based stress detector with blood pressure and body tempera...Fuzzy logic method-based stress detector with blood pressure and body tempera...
Fuzzy logic method-based stress detector with blood pressure and body tempera...
 
Autodesk Construction Cloud (Autodesk Build).pptx
Autodesk Construction Cloud (Autodesk Build).pptxAutodesk Construction Cloud (Autodesk Build).pptx
Autodesk Construction Cloud (Autodesk Build).pptx
 
Diploma Engineering Drawing Qp-2024 Ece .pdf
Diploma Engineering Drawing Qp-2024 Ece .pdfDiploma Engineering Drawing Qp-2024 Ece .pdf
Diploma Engineering Drawing Qp-2024 Ece .pdf
 
Maher Othman Interior Design Portfolio..
Maher Othman Interior Design Portfolio..Maher Othman Interior Design Portfolio..
Maher Othman Interior Design Portfolio..
 
Research Methodolgy & Intellectual Property Rights Series 1
Research Methodolgy & Intellectual Property Rights Series 1Research Methodolgy & Intellectual Property Rights Series 1
Research Methodolgy & Intellectual Property Rights Series 1
 
Interfacing Analog to Digital Data Converters ee3404.pdf
Interfacing Analog to Digital Data Converters ee3404.pdfInterfacing Analog to Digital Data Converters ee3404.pdf
Interfacing Analog to Digital Data Converters ee3404.pdf
 
Research Methodolgy & Intellectual Property Rights Series 2
Research Methodolgy & Intellectual Property Rights Series 2Research Methodolgy & Intellectual Property Rights Series 2
Research Methodolgy & Intellectual Property Rights Series 2
 
8th International Conference on Soft Computing, Mathematics and Control (SMC ...
8th International Conference on Soft Computing, Mathematics and Control (SMC ...8th International Conference on Soft Computing, Mathematics and Control (SMC ...
8th International Conference on Soft Computing, Mathematics and Control (SMC ...
 
Piping and instrumentation diagram p.pdf
Piping and instrumentation diagram p.pdfPiping and instrumentation diagram p.pdf
Piping and instrumentation diagram p.pdf
 
"United Nations Park" Site Visit Report.
"United Nations Park" Site  Visit Report."United Nations Park" Site  Visit Report.
"United Nations Park" Site Visit Report.
 
Dynamo Scripts for Task IDs and Space Naming.pptx
Dynamo Scripts for Task IDs and Space Naming.pptxDynamo Scripts for Task IDs and Space Naming.pptx
Dynamo Scripts for Task IDs and Space Naming.pptx
 
ALCOHOL PRODUCTION- Beer Brewing Process.pdf
ALCOHOL PRODUCTION- Beer Brewing Process.pdfALCOHOL PRODUCTION- Beer Brewing Process.pdf
ALCOHOL PRODUCTION- Beer Brewing Process.pdf
 
Linux Systems Programming: Semaphores, Shared Memory, and Message Queues
Linux Systems Programming: Semaphores, Shared Memory, and Message QueuesLinux Systems Programming: Semaphores, Shared Memory, and Message Queues
Linux Systems Programming: Semaphores, Shared Memory, and Message Queues
 
5G and 6G refer to generations of mobile network technology, each representin...
5G and 6G refer to generations of mobile network technology, each representin...5G and 6G refer to generations of mobile network technology, each representin...
5G and 6G refer to generations of mobile network technology, each representin...
 
litvinenko_Henry_Intrusion_Hong-Kong_2024.pdf
litvinenko_Henry_Intrusion_Hong-Kong_2024.pdflitvinenko_Henry_Intrusion_Hong-Kong_2024.pdf
litvinenko_Henry_Intrusion_Hong-Kong_2024.pdf
 
Worksharing and 3D Modeling with Revit.pptx
Worksharing and 3D Modeling with Revit.pptxWorksharing and 3D Modeling with Revit.pptx
Worksharing and 3D Modeling with Revit.pptx
 
NEWLETTER FRANCE HELICES/ SDS SURFACE DRIVES - MAY 2024
NEWLETTER FRANCE HELICES/ SDS SURFACE DRIVES - MAY 2024NEWLETTER FRANCE HELICES/ SDS SURFACE DRIVES - MAY 2024
NEWLETTER FRANCE HELICES/ SDS SURFACE DRIVES - MAY 2024
 

NEW BLENDED CEMENTS

  • 1. NEW BLENDED CEMENTS by Dr J D BAPAT www.drjdbapat.com INDIAN CEMENT REVIEW CONFERENCE 2014 on SUSTAINABILITY IN INDIAN CEMENT INDUSTRY 6 JUNE 2014, MUMBAI
  • 2. NEW BLENDED CEMENTS PRINCIPAL DEVELOPMENT GOALS  REDUCING CARBON (GHG) EMISSION THROUGH CLINKER SUBSTITUTION  REDUCING ENERGY CONSUMPTION  INCREASED PRODUCTION CAPACITY REDUCING SOLID WASTE  MAINTAINING QUALITY : STRENGTH & DURABILITY
  • 3. NEW BLENDED CEMENTS IS 456 – 2000 PROVISIONS ADMIXTURES PERMITTED BY INDIAN STANDARD CODE FOR PLAIN AND REINFORCED CONCRETE i.e. IS 456 – 2000  FLY ASH (15-35% )  BLAST FURNACE SLAG OR GGBS (25-70%)  SILICA FUME (3-10%)*  RICE HUSK ASH (25-30%)*  METAKAOLIN (10-25%)* * Recommended as per common practice
  • 4. NEW BLENDED CEMENTS  PORTLAND LIMESTONE CEMENT (PLC)  PORTLAND HIGH VOLUME FLY ASH CEMENT (PHFC)
  • 6. NEW BLENDED CEMENTS PORTLAND LIMESTONE CEMENT (PLC) INDIAN & INTERNATIONAL STANDARDS  INDIAN STANDARD IS 269 - 2013: PERMITS ADDITION OF LIMESTONE UPTO 5%, AS PERFORMANCE IMPROVER, IN OPC  EUROPEAN STANDARD EN 197-1 (2000):  5% LS ADDITION PERMITTED IN ALL 27 APPROVED TYPES, AS MINOR ADDITIONAL CONSTITUENT (MAC)  OUT OF THAT, 4 ARE PORTLAND LIMESTONE CEMENT, PERMITTING HIGHER ADDITIONS OF LS, IN ADDITION TO 5% MAC AS ABOVE  CEM II/A-L & CEM II/A-LL: 6 TO 20% & CEM II/B-L & CEM II/B-LL: 21-35%  US STANDARDS:  ASTM C150: 5% LS ADDITION PERMITTED IN TYPES I TO V  ASTM C595 & AASHTO M240: 5-15% LS ADDITION PERMITTED IN TYPE IL & IT CANADIAN STANDARD CSA A3001:  5% LS ADDITION PERMITTED IN PORTLAND CEMENT  6 - 15% LS ADDITION PERMITTED PORTLAND LIMESTONE CEMENT
  • 7. NEW BLENDED CEMENTS PORTLAND LIMESTONE CEMENT (PLC) SIGNIFICANCE OF 15% LIMIT Matschei et al. 2007
  • 8. NEW BLENDED CEMENTS PORTLAND LIMESTONE CEMENT (PLC) HOW LIMESTONE WORKS PARTICLE PACKING – IMPROVED PARTICLE SIZE DISTRIBUTION
  • 9. NEW BLENDED CEMENTS PORTLAND LIMESTONE CEMENT (PLC) HOW LIMESTONE WORKS PROVIDES NUCLEATION SURFACES FOR PRECIPITATION OF HYDRATED CEMENT
  • 10. NEW BLENDED CEMENTS PORTLAND LIMESTONE CEMENT (PLC) HOW LIMESTONE WORKS LS REACTS WITH ALUMINATES IN CEMENT TO FORM CARBOALUMINATES
  • 11. NEW BLENDED CEMENTS PORTLAND LIMESTONE CEMENT (PLC) LIMESTONE REQUIREMENTS: EN STANDARDS  CALCIUM CARBONATE > 75%  TOTAL ORGANIC CARBON (TOC): MAX 0.5%  CLAY: MAX 1.2 g/100g
  • 12. NEW BLENDED CEMENTS PORTLAND LIMESTONE CEMENT (PLC) PRODUCTION OF PLC  METERED PROPORTION OF CRUSHED, DRIED LS FED TO FINISH GRINDING MILL ALONG, WITH CLINKER & GYPSUM  LS IS MORE EASILY GROUND THAN CLINKER (HARDER) & GETS CONCENTRATED IN FINE PARTICLES  OVERALL FINENESS MUST BE HIGHER, FOR EQUIVALENT PERF (.) TO HAVE FINENESS OF THE CLINKER FRACTION TO BE SIMILAR TO OPC:  PRODUCTION RATE IS SLOWED  SOME ADDITIONAL GRINDING ENERGY REQUIRED BUT IS MORE THAN OFFSET BY LOWER CLINKER CONTENT & RELATED KILN FUEL SAVINGS  PARTICLE SIZE DISTRIBUTION IS ENHANCED  HYDRATION IS ENHANCED BY BOTH PHYSICAL AND CHEMICAL INTERACTION  SUSTAINABILITY BENEFITS SIGNIFICANT: REDUCED ASSOCIATED CARBON EMISSIONS & EMBODIED ENERGY (LESS CLINKER)
  • 13. NEW BLENDED CEMENTS PORTLAND LIMESTONE CEMENT (PLC) PRODUCTION PLC INTER-GRINDING WITH CLINKER GRINDING ENERGY CONSUMPTION DECREASES WITH LS REPLACEMENT Opoczky, L., 1992
  • 14. NEW BLENDED CEMENTS PORTLAND LIMESTONE CEMENT (PLC) FRESH CONCRETE WITH PLC  WATER DEMAND & WORKABILITY RELATED TO PARTICLE SIZE DISTRIBUTION OF LS IN RELATION TO CEMENT  GENERALLY INCREASED WATER IS NEEDED TO MAINTAIN CONSISTENCY OF CEMENT PASTES AS LS CONTENT INCREASES FINE LS PARTICLES ENHANCE OVERALL PARTICLE PACKING OF BINDER MATERIALS RESULTING IN LESS SPACE FOR WATER BETWEEN SOLID GRAINS DECREASING AVERAGE PARTICLE SIZE OF LS GIVES BETTER EARLY-AGE RHEOLOGICAL PROPERTIES
  • 15. NEW BLENDED CEMENTS PORTLAND LIMESTONE CEMENT (PLC) FRESH CONCRETE WITH PLC REDUCED BLEEDING Specific Surface Area m2/kg Building Research Establishment , 1993
  • 16. NEW BLENDED CEMENTS PORTLAND LIMESTONE CEMENT (PLC) FRESH CONCRETE WITH PLC HYDRATION  AS LIMESTONE ACTS AS NUCLEATION SITES FOR HYDRATION PRODUCTS ITS INCLUSION INCREASES RATE OF HYDRATION  LIMESTONE ADDITIONS GIVE EARLIER PEAK FOR HEAT OF HYDRATION
  • 17. NEW BLENDED CEMENTS PORTLAND LIMESTONE CEMENT (PLC) MECHANICAL PROPERTIES: CONCRETE WITH PLC  LS UP TO 5% INCREASES EARLY-AGE STRENGTH DUE TO: IMPROVED PARTICLE PACKING , INCREASED RATE OF CEMENT HYDRATION & EARLY PRODUCTION OF CALCIUM CARBOALUMINATE (.) APPLIES TO BOTH INTER-GROUND & BLENDED PLC  HIGHER REPLACEMENTS: LOSS OF STRENGTH DUE TO DILUTION MUST BE COMPENSATED BY FINER GRINDING (.) VOGLIS ET AL (2005): SHOWED COMPARABLE STRENGTHS FOR PC & PLC WITH 15% LS, WHEN PLC WAS GROUND TO 511 m2/kg COMPARED WITH 303 m2/kg FOR PC  TSIVILIS ET AL (1999): APPROPRIATE CHOICE OF CLINKER QUALITY, LS QUALITY, % LS CONTENT & CEMENT FINENESS CAN LEAD TO PRODUCTION OF PLC WITH DESIRED PROPERTIES, AT LEAST FOR CEMENTS WITH UP TO 15% LS  TENSILE, FLEXURAL STRENGTH & MODULUS OF ELASTICITY: STANDARD EQUATIONS APPLICABLE (.) SHRINKAGE SAME BUT CREEP INCREASES
  • 18. NEW BLENDED CEMENTS PORTLAND LIMESTONE CEMENT (PLC) DURABILITY OF CONCRETE WITH PLC CONCRETE PERMEABILITY Matthews, J.D. 1994.
  • 19. NEW BLENDED CEMENTS PORTLAND LIMESTONE CEMENT (PLC) DURABILITY OF CONCRETE WITH PLC CHLORIDE DIFFUSION COEFFICIENT Dhir, R.K., et.al. 2007.
  • 20. NEW BLENDED CEMENTS PORTLAND LIMESTONE CEMENT (PLC) DURABILITY OF CONCRETE WITH PLC CARBONATION Dhir, R.K., et.al. 2007
  • 21. NEW BLENDED CEMENTS PORTLAND LIMESTONE CEMENT (PLC) DURABILITY OF CONCRETE WITH PLC CARBONATION  IN REFERENCE TO HYDRATED PLC, STRENGTH OF PLC AFTER ACCELERATED CARBONATION WAS 79% HIGHER AT 28 D, EVEN THOUGH ULTIMATE LS CONTENT IN CARBONATED PLC WAS OVER 40%  CALCIUM CARBONATES PRODUCED BY ACCELERATED CARBONATION GETS IMBEDDED IN C-S-H, FORMING INTERMINGLED MICROSTRUCTURE  HIGH CARBONATION REACTIVITY OF PLC ATTRIBUTED TO FINE PARTICLE SIZE & EXISTENCE OF LS POWDER NUCLEI FOR CALCIUM CARBONATE PRECIPITATION  USE OF PLC IN ACCELERATED CARBONATION OF CONCRETE PRODUCTS CAN SIGNIFICANTLY CONTRIBUTE TO A NET GAIN IN STRENGTH & CARBON EMISSION REDUCTION Ref: Shao Y., et. al. 2014
  • 22. NEW BLENDED CEMENTS PORTLAND LIMESTONE CEMENT (PLC) DURABILITY OF CONCRETE WITH PLC SULPHATE RESISTANCE  STANDARDS DO NOT RECOMMEND USE OF PLC IN SULPHATE ENVIRONMENT  AT NORMAL TEMPERATURE, SULPHATE RESISTANCE OF PLC IS SUBSTANTIALLY IMPROVED WHEN 30-50% SLAG IS ADDED & LS REPLACEMENT OF 5-15% ARE ALLOWABLE  SIMILARLY AT 5 C ALSO, SULPHATE RESISTANCE IS SUBSTANTIALLY IMPROVED WITH THE ADDITION OF SLAG Ref: Ramezanianpour A. M., 2012
  • 23. NEW BLENDED CEMENTS PORTLAND LIMESTONE CEMENT (PLC) DURABILITY OF CONCRETE WITH PLC OTHER DURABILITY PARAMETERS  SALT SCALING & FREEZE-THAW: LIMITED DATA AVAILABLE FOR AIR- ENTRAINED CONCRETE SHOW THAT FREEZE-THAW & SALT SCALING RESISTANCE OF PLC CONCRETE IS COMPARABLE TO THAT OF EQUIVALENT PC CONCRETE  ABRASION RESISTANCE: CONCRETES OF IDENTICAL 28-DAY STRENGTH HAVE SIMILAR ABRASION RESISTANCE, IRRESPECTIVE OF LS CONTENT OF CEMENT
  • 24. NEW BLENDED CEMENTS PORTLAND LIMESTONE CEMENT (PLC) SUMMARY  LS CEMENTS HAVE BEEN USED IN MANY COUNTRIES SINCE THE 1960’S & EU CEM II/A 6 TO 20% LIMESTONE CEMENTS ARE THE LARGEST SINGLE TYPE OF CEMENT CURRENTLY PRODUCED IN EUROPEAN COUNTRIES  LS FINENESS & PARTICLE SIZE DISTRIBUTION ARE KEY PARAMETRS ADVANTAGES:  PLC RESULTS IN REDUCED GHG EMISSIONS  WHEN PROPERLY OPTIMISED, PLC CONCRETE HAS FRESH PROPERTIES, BLEEDING & STRENGTH SIMILAR TO OPC CONCRETE REDUCED PERMEABILITY  SIMILAR CHLORIDE DURABILITY UP TO 15% REPLACEMENT  SIMILAR CARBONATION RATE UP TO 15% REPLACEMENT, AT LOW W/C RATIO  SUBSTANTIALLY IMPROVED SULPHATE RESISTANCE, WHEN PLC UP TO 15% LS, IS BLENDED WITH SLAG WITH 50% REPLACEMENT DISADVANTAGE:  PERFORMANCE IS AFFECTED BY (A) QUALITY OF LS, (B) WHETHER INTERGROUND OR BLENDED & (C) PARTICLE SIZE DISTRIBUTION
  • 25. PORTLAND HIGH VOLUME FLY ASH CEMENT PHFC
  • 26. NEW BLENDED CEMENTS PORTLAND HIGH VOLUME FLY ASH CEMENT (PHFC) PHFC REFERS TO BLENDED CEMENT PRODUCED IN CEMENT PLANT, WITH FA REPLACEMENT CEMENT >55% AT PRESENT HIGH VOLUMES OF FA (>55%) ARE ADDED AS REPLACEMENT OF CEMENT, AT RMC PLANTS, TO PRODUCE HIGH VOLUME FLY ASH CONCRETE (HVFAC) (.) IT NECESSITATES ADDITIONAL STORAGE SILOS & QUALITY CONTROL AT JOB SITE PHFC IS ONE OPTION, INCREASING AMOUNT OF FA THAT CAN REPLACE PORTLAND CEMENT (PC) FROM <20% IN CONVENTIONAL MIXES UP TO AS HIGH AS 55% PHFC CAN BE PRODUCED EITHER BY INTER-GRINDING FA WITH PC CLINKER & GYPSUM OR BY BLENDING DRY FA WITH PC (.) SOMETIMES DRY SUPER PLASTICISER IS ALSO INTERGROUND (.) PRODUCTION OF PHFC USING INTER-GRINDING METHOD APPEARS MOST COST-EFFECTIVE & PRACTICAL REQUIRED TO SATISFY MINIMUM STRENGTH AS PER ASTM C1157, OF 10 & 17 MPa AT 3 & 7 DAYS RESPECTIVELY
  • 27. NEW BLENDED CEMENTS PORTLAND HIGH VOLUME FLY ASH CEMENT (PHFC) WHY INTER-GRINDING EFFECT OF GRINDING ON FA PROPERTIES  SPECIFIC GRAVITY: INCREASES DUE TO CRUSHING OF PLEROSHERES AND CENOSHERES AND CONTUES FOR CERTAIN TIME PERIOD OF GRINDING  SPECIFIC SURFACE: INCREASES WITH GRINDING TIME, BUT AT THE EXPENSE OF GRINDING ENERGY  MORPHOLOGY: OPTIMUM GRINDING PERIOD DOES NOT AFFECT SPHERICAL SHAPE OF FA PARTICLES SIGNIFICANTLY  WATER REQUIREMENT OF MORTAR: DECREASES UP TO CERTAIN TIME PERIOD & LATER INCREASES (.) RELATED TO SPHERICAL SHAPE  POZZOLANIC ACTIVITY: INCREASES AT RAPID RATE UP TO CERTAIN TIME PERIOD, LATER RATE DECREASES  THESE ASPECTS SHOW PHFC SHOULD BE PREFERABLY PRODUCED BY INTER-GRINDING & GRINDING PERIOD SHOULD BE OPTIMISED.
  • 28. NEW BLENDED CEMENTS PORTLAND HIGH VOLUME FLY ASH CEMENT (PHFC) GRINDING SUPERPLASTICISER WITH CLINKER & GYPSUM WHEN NAPHTHALINE BASED SP WAS VARIED FROM 0-0.9% (MASS OF CLINKER+GYPSUM):  GRINDING TIME: SP ACTED AS GRINDING AID & GRINDING TIME REDUCED TO OBTAIN REQUIRED BLAINE FINENESS  WATER REQUIREMENT & COMPRESSIVE STRENGTH: SP ADDITION DURING GRINDING OR SEPARATELY AT THE MIXER PRODUCED SAME EFFECT  BLAINE: FIXED ON THE BASIS OF FA, BY CARRYING OUT TRIALS  BETTER TO ADD SP AT THE GRINDING STAGE  ADDITION OF SP ALSO ELIMINATES COMPATIBILITY ISSUES AT CONCRETING STAGE  PREDETERMINED QUANTITY OF SP MAY BE ADDED TO OBTAIN REQUIRED CONCRETE SLUMP
  • 29. NEW BLENDED CEMENTS PORTLAND HIGH VOLUME FLY ASH CEMENT (PHFC) CONCRETE WITH PHFC RESULTS OF LABORATORY TRIALS ON PHFC WITH 55% FA*  FRESH CONCRETE: CONCRETE WITH PHFC REQUIRED MORE SP & AEA, AS INTER-GRINDING INCREASED FINENESS  COMPRESSIVE STRENGTH: IRRESPECTIVE OF SOURCE & TYPE OF FA, CONCRETE WITH PHFC DEVELOPED BETTER STRENGTH COMPARED TO THAT PREPARED BY SEPARATE ADDITION OF CEMENT & UN-GROUND FA AT MIXER  CHLORIDE RESISTANCE: INTER-GRINDING IMPROVED CHLORIDE RESISTANCE OF CONCRETE *Ref: Electric Power Research Institute (EPRI), USA, 2001
  • 30. NEW BLENDED CEMENTS PORTLAND HIGH VOLUME FLY ASH CEMENT (PHFC) SUMMARY PHFC IS FACTORY MADE WITH FA REPLACING CEMENT AT 55% ADDING SP TO CLINKER AT FINISH GRINDING STAGE HELP REDUCE GRINDING ENERGY & ALSO SOLVES COMPATIBILITY ISSUES AT CONCRETING STAGE INTER-GRINDING FA WITH GROUND CEMENT FOR FIXED TIME PERIOD IMPARTS BETTER CONCRETE PROPERTIES PHFC HAS VERY GOOD RESISTANCE TOWARDS CHLORIDE PENETRATION
  • 31. NEW BLENDED CEMENTS  NO CEMENT OR ADMIXTURE CAN OFFSET LOW QUALITY CONCRETE  DURABLE CONCRETE DEPENDS ON:  APPROPRIATE MIXTURE PROPORTIONS  LOWER w/c RATIO  PROPER PLACEMENT  CURING  MAINTENANCE  WHEN GOOD PRACTICES ARE FOLLOWED, CONCRETE WILL ATTAIN ITS EXPECTED SERVICE LIFE
  • 32. JOIN MY NETWORK YOU ARE WELCOME TO JOIN ME  FACEBOOK: Jayant D Bapat  TWITTER: @cemcretecon & @drjdbapat  LINKEDIN: Dr J. D. Bapat (email: jdbapat@yahoo.co.in)  EMAIL_1: consult@drjdbapat.com  EMAIL_2: consult.bapat@yahoo.com  URL: http://www.drjdbapat.com