The document discusses the various stages of the dental casting procedure, including both clinical and laboratory steps. It begins with tooth preparation and making an impression in the clinical stage. In the laboratory, a die is prepared from the impression and a wax pattern is fabricated on the die. The wax pattern is then invested and the wax eliminated to create a mold, into which molten alloy is cast to produce a dental restoration. The document provides details on materials, techniques and historical developments related to each step of the lost wax casting process.
A STEP IN CASTING OF CAST PARTIAL DENTURE, a precious duplication process and proper wax up of refractory cast results in accurate fitting of the framework of the prosthesis.
A STEP IN CASTING OF CAST PARTIAL DENTURE, a precious duplication process and proper wax up of refractory cast results in accurate fitting of the framework of the prosthesis.
a detailed account of the principles of tooth preparation with main reference from Shillingburg
The presentation is available on request. Mail me at apurvathampi@gmail.com
This presentation provide brief information about different types of cements in Dentistry. also you will find information about cementation tips and techniques. Recent resin cements are also included in this presentation
A RPD derives support from two main sources periodontally sound natural teeth & residual alveolar processes and associated soft tissues.
A RPD that is supported by healthy natural teeth possesses adequate stability and retention to resist functional displacement.
However, a RPD that is not entirely bounded by natural teeth will move when a load is applied.
Inlays and onlays / implant dentistry course/ implant dentistry courseIndian dental academy
Indian Dental Academy: will be one of the most relevant and exciting training center with best faculty and flexible training programs for dental professionals who wish to advance in their dental practice,Offers certified courses in Dental implants,Orthodontics,Endodontics,Cosmetic Dentistry, Prosthetic Dentistry, Periodontics and General Dentistry.
a detailed account of the principles of tooth preparation with main reference from Shillingburg
The presentation is available on request. Mail me at apurvathampi@gmail.com
This presentation provide brief information about different types of cements in Dentistry. also you will find information about cementation tips and techniques. Recent resin cements are also included in this presentation
A RPD derives support from two main sources periodontally sound natural teeth & residual alveolar processes and associated soft tissues.
A RPD that is supported by healthy natural teeth possesses adequate stability and retention to resist functional displacement.
However, a RPD that is not entirely bounded by natural teeth will move when a load is applied.
Inlays and onlays / implant dentistry course/ implant dentistry courseIndian dental academy
Indian Dental Academy: will be one of the most relevant and exciting training center with best faculty and flexible training programs for dental professionals who wish to advance in their dental practice,Offers certified courses in Dental implants,Orthodontics,Endodontics,Cosmetic Dentistry, Prosthetic Dentistry, Periodontics and General Dentistry.
Recent advances in dental porcelain materials / cosmetic dentistry coursesIndian dental academy
The Indian Dental Academy is the Leader in continuing dental education , training dentists in all aspects of dentistry and
offering a wide range of dental certified courses in different formats.
The Indian Dental Academy is the Leader in continuing dental education , training dentists in all aspects of dentistry and
offering a wide range of dental certified courses in different formats.for more details please visit
www.indiandentalacademy.com
Evolution of casting machines final /orthodontic courses by Indian dental aca...Indian dental academy
The Indian Dental Academy is the Leader in continuing dental education , training dentists in all aspects of dentistry and
offering a wide range of dental certified courses in different formats.for more details please visit
www.indiandentalacademy.com
Indian Dental Academy: will be one of the most relevant and exciting training
center with best faculty and flexible training programs for dental
professionals who wish to advance in their dental practice,Offers certified
courses in Dental implants,Orthodontics,Endodontics,Cosmetic Dentistry,
Prosthetic Dentistry, Periodontics and General Dentistry.
Dental ceramics /certified fixed orthodontic courses by Indian dental academy Indian dental academy
Welcome to Indian Dental Academy
The Indian Dental Academy is the Leader in continuing dental education , training dentists in all aspects of dentistry and offering a wide range of dental certified courses in different formats.
Indian dental academy has a unique training program & curriculum that provides students with exceptional clinical skills and enabling them to return to their office with high level confidence and start treating patients
State of the art comprehensive training-Faculty of world wide repute &Very affordable.
Dental ceramics/certified fixed orthodontic courses by Indian dental academy Indian dental academy
The Indian Dental Academy is the Leader in continuing dental education , training dentists in all aspects of dentistry and
offering a wide range of dental certified courses in different formats
Welcome to TechSoup New Member Orientation and Q&A (May 2024).pdfTechSoup
In this webinar you will learn how your organization can access TechSoup's wide variety of product discount and donation programs. From hardware to software, we'll give you a tour of the tools available to help your nonprofit with productivity, collaboration, financial management, donor tracking, security, and more.
Macroeconomics- Movie Location
This will be used as part of your Personal Professional Portfolio once graded.
Objective:
Prepare a presentation or a paper using research, basic comparative analysis, data organization and application of economic information. You will make an informed assessment of an economic climate outside of the United States to accomplish an entertainment industry objective.
The Roman Empire A Historical Colossus.pdfkaushalkr1407
The Roman Empire, a vast and enduring power, stands as one of history's most remarkable civilizations, leaving an indelible imprint on the world. It emerged from the Roman Republic, transitioning into an imperial powerhouse under the leadership of Augustus Caesar in 27 BCE. This transformation marked the beginning of an era defined by unprecedented territorial expansion, architectural marvels, and profound cultural influence.
The empire's roots lie in the city of Rome, founded, according to legend, by Romulus in 753 BCE. Over centuries, Rome evolved from a small settlement to a formidable republic, characterized by a complex political system with elected officials and checks on power. However, internal strife, class conflicts, and military ambitions paved the way for the end of the Republic. Julius Caesar’s dictatorship and subsequent assassination in 44 BCE created a power vacuum, leading to a civil war. Octavian, later Augustus, emerged victorious, heralding the Roman Empire’s birth.
Under Augustus, the empire experienced the Pax Romana, a 200-year period of relative peace and stability. Augustus reformed the military, established efficient administrative systems, and initiated grand construction projects. The empire's borders expanded, encompassing territories from Britain to Egypt and from Spain to the Euphrates. Roman legions, renowned for their discipline and engineering prowess, secured and maintained these vast territories, building roads, fortifications, and cities that facilitated control and integration.
The Roman Empire’s society was hierarchical, with a rigid class system. At the top were the patricians, wealthy elites who held significant political power. Below them were the plebeians, free citizens with limited political influence, and the vast numbers of slaves who formed the backbone of the economy. The family unit was central, governed by the paterfamilias, the male head who held absolute authority.
Culturally, the Romans were eclectic, absorbing and adapting elements from the civilizations they encountered, particularly the Greeks. Roman art, literature, and philosophy reflected this synthesis, creating a rich cultural tapestry. Latin, the Roman language, became the lingua franca of the Western world, influencing numerous modern languages.
Roman architecture and engineering achievements were monumental. They perfected the arch, vault, and dome, constructing enduring structures like the Colosseum, Pantheon, and aqueducts. These engineering marvels not only showcased Roman ingenuity but also served practical purposes, from public entertainment to water supply.
Honest Reviews of Tim Han LMA Course Program.pptxtimhan337
Personal development courses are widely available today, with each one promising life-changing outcomes. Tim Han’s Life Mastery Achievers (LMA) Course has drawn a lot of interest. In addition to offering my frank assessment of Success Insider’s LMA Course, this piece examines the course’s effects via a variety of Tim Han LMA course reviews and Success Insider comments.
June 3, 2024 Anti-Semitism Letter Sent to MIT President Kornbluth and MIT Cor...Levi Shapiro
Letter from the Congress of the United States regarding Anti-Semitism sent June 3rd to MIT President Sally Kornbluth, MIT Corp Chair, Mark Gorenberg
Dear Dr. Kornbluth and Mr. Gorenberg,
The US House of Representatives is deeply concerned by ongoing and pervasive acts of antisemitic
harassment and intimidation at the Massachusetts Institute of Technology (MIT). Failing to act decisively to ensure a safe learning environment for all students would be a grave dereliction of your responsibilities as President of MIT and Chair of the MIT Corporation.
This Congress will not stand idly by and allow an environment hostile to Jewish students to persist. The House believes that your institution is in violation of Title VI of the Civil Rights Act, and the inability or
unwillingness to rectify this violation through action requires accountability.
Postsecondary education is a unique opportunity for students to learn and have their ideas and beliefs challenged. However, universities receiving hundreds of millions of federal funds annually have denied
students that opportunity and have been hijacked to become venues for the promotion of terrorism, antisemitic harassment and intimidation, unlawful encampments, and in some cases, assaults and riots.
The House of Representatives will not countenance the use of federal funds to indoctrinate students into hateful, antisemitic, anti-American supporters of terrorism. Investigations into campus antisemitism by the Committee on Education and the Workforce and the Committee on Ways and Means have been expanded into a Congress-wide probe across all relevant jurisdictions to address this national crisis. The undersigned Committees will conduct oversight into the use of federal funds at MIT and its learning environment under authorities granted to each Committee.
• The Committee on Education and the Workforce has been investigating your institution since December 7, 2023. The Committee has broad jurisdiction over postsecondary education, including its compliance with Title VI of the Civil Rights Act, campus safety concerns over disruptions to the learning environment, and the awarding of federal student aid under the Higher Education Act.
• The Committee on Oversight and Accountability is investigating the sources of funding and other support flowing to groups espousing pro-Hamas propaganda and engaged in antisemitic harassment and intimidation of students. The Committee on Oversight and Accountability is the principal oversight committee of the US House of Representatives and has broad authority to investigate “any matter” at “any time” under House Rule X.
• The Committee on Ways and Means has been investigating several universities since November 15, 2023, when the Committee held a hearing entitled From Ivory Towers to Dark Corners: Investigating the Nexus Between Antisemitism, Tax-Exempt Universities, and Terror Financing. The Committee followed the hearing with letters to those institutions on January 10, 202
The French Revolution, which began in 1789, was a period of radical social and political upheaval in France. It marked the decline of absolute monarchies, the rise of secular and democratic republics, and the eventual rise of Napoleon Bonaparte. This revolutionary period is crucial in understanding the transition from feudalism to modernity in Europe.
For more information, visit-www.vavaclasses.com
Acetabularia Information For Class 9 .docxvaibhavrinwa19
Acetabularia acetabulum is a single-celled green alga that in its vegetative state is morphologically differentiated into a basal rhizoid and an axially elongated stalk, which bears whorls of branching hairs. The single diploid nucleus resides in the rhizoid.
Model Attribute Check Company Auto PropertyCeline George
In Odoo, the multi-company feature allows you to manage multiple companies within a single Odoo database instance. Each company can have its own configurations while still sharing common resources such as products, customers, and suppliers.
A Strategic Approach: GenAI in EducationPeter Windle
Artificial Intelligence (AI) technologies such as Generative AI, Image Generators and Large Language Models have had a dramatic impact on teaching, learning and assessment over the past 18 months. The most immediate threat AI posed was to Academic Integrity with Higher Education Institutes (HEIs) focusing their efforts on combating the use of GenAI in assessment. Guidelines were developed for staff and students, policies put in place too. Innovative educators have forged paths in the use of Generative AI for teaching, learning and assessments leading to pockets of transformation springing up across HEIs, often with little or no top-down guidance, support or direction.
This Gasta posits a strategic approach to integrating AI into HEIs to prepare staff, students and the curriculum for an evolving world and workplace. We will highlight the advantages of working with these technologies beyond the realm of teaching, learning and assessment by considering prompt engineering skills, industry impact, curriculum changes, and the need for staff upskilling. In contrast, not engaging strategically with Generative AI poses risks, including falling behind peers, missed opportunities and failing to ensure our graduates remain employable. The rapid evolution of AI technologies necessitates a proactive and strategic approach if we are to remain relevant.
Operation “Blue Star” is the only event in the history of Independent India where the state went into war with its own people. Even after about 40 years it is not clear if it was culmination of states anger over people of the region, a political game of power or start of dictatorial chapter in the democratic setup.
The people of Punjab felt alienated from main stream due to denial of their just demands during a long democratic struggle since independence. As it happen all over the word, it led to militant struggle with great loss of lives of military, police and civilian personnel. Killing of Indira Gandhi and massacre of innocent Sikhs in Delhi and other India cities was also associated with this movement.
Instructions for Submissions thorugh G- Classroom.pptxJheel Barad
This presentation provides a briefing on how to upload submissions and documents in Google Classroom. It was prepared as part of an orientation for new Sainik School in-service teacher trainees. As a training officer, my goal is to ensure that you are comfortable and proficient with this essential tool for managing assignments and fostering student engagement.
3. CONTENTS
INTRODUCTION
DEFINITIONS
HISTORY
STAGES OF CASTING PROCEDURE:
I) CLINICAL STEPS : 1) TOOTH PREPARATION
2) MAKING OF THE IMPRESSION
II) LABORATORY STEPS:
3) PREPARATION OF DIE OR CAST
4) WAX PATTERN PREPARATION
5) SPRUE FORMER & SPRUING
6) CASTING RING & RING LINERS
7) INVESTING
8) WAX ELIMINATION OR BURN OUT
9)CRUCIBLES
10) METHODS OF MELTING ALLOYS
11) CASTING MACHINES
12) CLEANING & FINISHING THE CASTING
CASTING DEFECTS 3
4. INTRODUCTION
Casting is one the most widely used methods for fabrication of metallic
restorations outside the mouth.
The technique of investment casting is both one of the oldest & most advanced
of the metallurgical arts.
The lost wax casting technique was 1st described at the end of 19th century as a
means of making dental castings.
The process consists of surrounding the wax pattern with a mold made of heat
resistant investment material, eliminating the wax by heating and then
introducing the molten metal into the mold through a channel called “Sprue”.
4
6. In Dentistry, the resulting casting must be a highly accurate replica of wax
pattern with surface details & accurate dimensions.
Small variations in investing or casting can significantly affect the quality of
final restoration.
Successful casting depends on accuracy & consistency of technique.
We are going to know the exact influence of each variable in the technique & to
make rationale changes to modify the technique according to need.
6
7. DEFINITIONS
1) ACCORDING TO GPT (7th edition): Casting is defined as something that has
been cast in a mold, an object formed by the solidification of a fluid that has
been poured or injected into a mold.
2) ACCORDING TO CRAIG (12th Edition): Casting is the process by which a wax
pattern of a restoration is converted to a replicate in a dental alloy.
3) ACCORDING TO WILLIAM J. OBRIEN (3rd edition): Casting is a process of
forming objects by pouring molten metals in molds that are cooled to cause
solidification.
7
8. 4) CASTING PROCEDURE: It is a process of obtaining a metallic duplicate of a
missing tooth structure by pouring molten metal into a mold of a required
form & allowing it to solidify to obtain a metallic duplicate.
5) LOST WAX TECHNIQUE: It is so named because a wax pattern of a
restoration is invested in a ceramic material, then the pattern is burned out
(“Lost”) to create a space into which molten metal is placed or cast.
6) CASTABILITY: The ability of an alloy to completely fill a mold.
8
9. .
OBJECTIVE OF CASTING PROCEDURE :
To provide a metallic duplication of the missing tooth
structure , with as much accuracy as possible .
9
10. “Lost Wax” Method dates back to atleast 4th millenium B.C.
Dental casting procedures have originated from Black smithery which dates
back to the early civilizations of Mesopotamia to Egypt where Utensils,
Weapons & Tools were cast in Brass alloys using simple techniques.
Remarkably, civilizations as diverse as China’s Han Dynasty, the Benin kingdom
in Africa & the Aztecs of pre-columbian Mexico employed similar techniques.
The use of dental casting machines to fabricate cast metal restoration is
credited to the people of the early chinese civilization in the Bronze age.
Dental castings were first seen in the Skulls of people of the Chinese civilization
where cast metal restorations were fastened onto the human teeth, with metal
wires passing through the space between the teeth.
HISTORY
10
12. 11th Century Theophilus Described lost wax technique, which was a
common practice prevailed in 11th century.
1558 Benvenuto Cellini Claimed to have attempted, use of wax and clay for
preparation of castings.
Cast his bronze masterpiece “Perseus & the Head of Medusa” using the Lost
wax process.
1884 Agulihon de saran Used 24K gold to form Inlay
1887 J. R. Knapp Invented Blowpipe
1897 Philbrook Described a method of casting metal filling.
12
13. -The casting procedure by the Lost wax technique was introduced by
Dr.William H.Taggart .
-Introduced this technique and the casting machine in 1907 before the
New York Odontological group .
1907 Taggart Devised a practically useful casting machine.
13
14. Gold melted with a blowpipe was then forced into the plaster mold by
means of casting machine, which utilized compressed air.
Inlay Mold
Blowpipe
Compressed air
cylinder
14
15. LANE – Suggested the idea of casting by using investment containing high
percentage of Silica to plaster of paris at 650 degrees c. to compensate for
casting shrinkage.
1910 – Von Horn introduced a different method of compensation- wax pattern
investmentequal to mouth temperature using high silica content investment.
1932 – SCHEN developed a technique employing hygroscopic expansion of
investment to compensate for shrinkage of casting.
1933 – Base Metal Alloys for RPD.
1942 – SONDER recognised that thermal expansion of investment was greatly
inhibited by metal casting ring & advocated lining the ring with soft asbestos.
15
16. 1950-Development of resin veneers for gold alloys
1959-Porcelain fused to metal technique
1968 – Palladium Alloys for Gold Alloy.
1970 – Ni-Cr Alloys for RPD, FPD.
1971 – The Gold Standard.
1977 - B.G. Waterstrat et al produced the world’s first Ti dental casting .
16
17. 1978 - Wilmer B. Eames and John F. MacNamara concluded that:
• Vacuum casting machines produced sharper margins than the centrifugal
casting machines.
1980 – All Ceramic Technologies.
1984 – Classification of Casting Alloys.
17
18. 1985 - T.E. Donovan and L.E. White studied the increase in castability of an
alloy by increasing the rate of acceleration of the centrifugal casting machine.
Waterstrat designed, split-chamber argon-vacuum casting equipment .
1989 - H. Hamanaka, H. Doi et al devised a new casting machine for dental
casting of titanium and Ni-Ti alloys
1990 - Arturo R. Hruska introduced the Titanium Decontaminator, a device
which decontaminates the mold before the actual process of casting was
carried out.
1999 – Gold alloys for Palladium alloys.
2002 – ADA proposals for mechanical properties
18
19. STAGES OF CASTING PROCEDURE
I) CLINICAL STEPS:
1. TOOTH PREPARATION: Preparation of the tooth structure to
receive the cast restoration.
19
20. TOOTH PREPARATION FOR INLAY CAST RESTORATION
Wall’s proper Facial & lingual walls parallel to the long axis of crown
Occlusal bevel 30-45 degrees to long axis of crown on outer plane of walls.
Flat pulpal floor
Axial wall Flat or slightly rounded in bucco-lingual direction
Gingival floor Flat in bucco-lingual direction
20
21. 2. MAKING OF IMPRESSION
- Impression of the prepared tooth structure.
- Indirect technique fabricating cast restorations.
OBJECTIVES OF IMPRESSIONS FOR INDIRECT FABRICATION OF CAST
RESTORATIONS:
- Record most finite details
- Duplicate unprepared surface areas beyond peripheries of preparation
- Dulplicate surface anatomy of adjacent & opposing teeth.
- Duplicate surface anatomy of adjacent soft tissues.
21
22. TYPES OF IMPRESSION MATERIALS CHOOSEN
Reversible agar hydrocolloid
Irreversible Alginate hydrocolloid
Polysulfide rubber base
Condensation polymerization silicone rubber base
Additional polymerization silicone rubber base
Polyether rubber bases
22
23. 3. PREPARATION OF MASTER DIE OR CAST
A die or cast is formed which is a duplicate of the intra oral structure.
(or)
The positive reproduction of the impression involving only the prepared tooth
for the processing of inlays or bridge structures.
A) REQUIREMENTS OF AN IDEAL DIE MATERIAL
1.Accuracy & Dimensional stability .
2. Reproducibility of fine detail .
3. Producing a smooth , hard surface .
4. Strength , resistance to shearing force , edge strength & abrasion resistance .
5 . Ease of manipulation . 23
24. B) MOST COMMONLY USED MATERIALS ARE:
Certified Type IV improved stone with S.E. of 0.1% or less.
Certified Type V improved stone with S.E. of 0.3%.
Electroformed dies
Epoxy resins
ADVANTAGES:
Easy to use
Inexpensive
Compatible with most of the impression materials.
24
26. C) METHODS OF ALTERING DIE DIMENSIONS:
- Addition of Accelerator or Retarder can be added to Type IV Stone to reduce its
S.E. < 0.1% & to reduce the diameter of the die.
GYPSUM DIES ARE SOMETIMES MODIFIED:
- Make more abrasion resistant.
- Change the dimensions of the dies.
- Increase the refractoriness of the dies.
TO INCREASE THE ABRASION RESISTANCE:
- Silver coating
- Coat the surface with cyanoacrylate &
- Adding the die hardener to the gypsum.
26
28. D) DIE LUBRICANTS:
- To avoid sticking of wax pattern to die.
INDICATIONS:
- Easy removal of casting from die.
28
29. E) DIE SPACER:
To produce relief space for cement.
Film thickness- 25microns
Applied in several coats to within 0.5mm of the preparation finish
line to provide relief for the cement luting agent.
MATERIALS USED:
• Mostly resins are used.
• Model paint
• Colored nail polish
• Thermoplastic polymers dissolved in
volatile solvents.
29
31. 4. WAX PATTERN PREPARATION
• 1st procedure in the casting of an inlay or crown for the lost-wax process is the
preparation of a dental wax pattern.
• Direct Wax Technique – Pattern made within the tooth.
Indirect Wax Technique – Pattern prepared within a die.
INLAY WAX – Specialized dental wax applied on the die surface for preparation of
direct & indirect patterns - Lost Wax Technique – Casting metals & Hot
pressing of ceramics.
American National Standards Institute / American Dental Association Sp No 4:
Type I – Medium Wax – Direct techniques .
Type II – Soft Wax – Indirect techniques . 31
33. Accurate reproduction of missing tooth structure.
Forms outline of the mold into which molten metal is poured.
A) COMPOSITION OF INLAY WAX:
Paraffin wax
Gum Dammar
Carnauba wax
Candelillia wax
Ceresin
Bees wax
Colouring agent
33
34. PARAFFIN WAX
-40-60%
• Derived from high boiling fractions of petroleum
• Complex mixture of hydrocarbons of methane series & Amorphous or
Microcrystalline phases .
• Type I always – paraffin- high melting point.
DISADVANTAGES:
• Flakes when it is trimmed
• No smooth, glossy surface.
34
35. GUM DAMMAR
• Natural resin
• Improves the smoothness in molding
• Increased resistance to cracking and flaking
• Increases toughness
• Enhances smoothness and lusture of the surface.
35
36. CARNAUBA WAX
• Fine powder leaves of tropical palms .
• Hard
• High melting point
• Decreases the flow at oral temperature
• Agreeable odour
• Contributes to the glossiness of wax surface
Replacements of Carnauba wax :
Complex nitrogen derivatives of higher fatty acids
Esters of acids derived from montan wax . 36
37. CANDELILLA WAX
Partially or entirely replace carnauba wax.
CERESIN
Modify – Toughness & Carving characteristics of the wax.
37
38. B. DESIRABLE PROPERTIES OF INLAY WAX:
Uniformity
Color contrast
Completely rigid and dimensionally stable at all times until eliminated
No Flakiness when bent and molded after softening
Wax pattern has solidifed – carve wax at margins – conform to surface of the
die.
ANSI/ADA Sp.No: 4
Melted wax when vapourised at 500C (932F) shall leave no residue in Excess of
0.10% of the original weight of the specimen .
38
39. C) FLOW
Type I – 37C (98F) is 1%
Type II - 9%
Minimizes distortion of a well Carved pattern as it is withdrawn from an
adequately tapered cavity in the tooth .
Min 70%-Max 90% at 45C
39
40. D) THERMAL PROPERTIES
Low thermal conductivity – More time is required to both heat them uniformly
and cool them to body temperature .
Thermal expansion data : Maximal TE allowed Between –
0.7% - Expansion with an inc. in temp. of 20 degrees from 37degrees.
0.35% - Contraction - Cooled from 37degrees - 25degrees
Average Linear coeffecient of Thermal expansion :
– 350 x 10-6/degreecentigrade
40
42. INTERPRETATION & CLINICAL IMPORTANCE :
GLASS TRANSITION TEMPERATURE: Temperature at which change in
expansion rate occurs .
- Rate of expansion increases abruptly above 35 degree (95 degrees F) .
- On completion of wax pattern , its removal from the tooth cavity and
Transfer to the lab bring about a reduction in temperature and subsequent
thermal contraction .
“A decrease of 12 degrees to 13degrees in temperature , from mouth
temperature to a room temperature of approx 24 degrees , causes a 0.4% linear
contraction of the wax , or about o.04% change for each degree change in
temperature . “
42
43. E. MANIPULATION
Methods of softening wax :
1. Best method – Controlled temperature oven .
Why ? Since it’s a poor thermal conductor , a controlled heating device for a
prolonged period ensures uniform softening .
2 . Dry heat – FLAME is preferred
- Twirled in the flame ? Always quick heating tends to melt the only the
superficial layer . So , this will bring inner surface out Vice versa .
- Repeat till the wax is warm all over .
- Knead it and shape it the prepared cavity .
43
44. 3 . Hot water bath – Inclusion of water droplets .
4 . Swaging – The die and the softened wax in the die are mounted into a
closed vessel containing water and a piston . When pressed , hydrostatic
pressure is evenly applied over the pattern to adapt it to the cavity .
44
45. According to Marzouk:
1. Formulation of a wax pattern by carving – Wax is overfilled & carved.
2. Incremental build-up of the wax pattern
3. Direct wax pattern
4. Anatomic core wax pattern
45
47. No 7 or 7 A Waxing spatula – Large increments .
Technique :
- Heat the instrument .
- Touch the wax .
- Quickly reheat the shank
47
48. G. CARVING
Sharp instruments .
And never heat it
Use light pressure .
Always overfill and carve.
Hold the carvers partly over the remaining tooth structure and
complete the carving with this guide .
48
49. PKT No 4
NO 2 WARD CARVERS NO1/2 & 3 HOLLENBACK CARVERS
PKT No 5
49
50. H. BURNISHING
- Slightly warm a blunt instrument and rub the wax , not as hot as it melts .
- Less effective than carving but easier to control and leaves a smoother surface
( esp. near margins ).
-Final polish with a silk cloth .
- In inaccessible areas , cotton wrapped around a toothpick .
50
52. I. REMOVAL OF WAX PATTERN
DIRECT PATTERN:
Sprue former Attached to the pattern Removed directly in line with its path
of withdrawl .
- Hook it with an explorer point and rotate it out of the cavity .
- In a MOD use a staple pin . Fasten it and insert a floss and hook it .
-Avoid finger contact it may produce a temperature rise .
INDIRECT PATTERNS:
- Lubricate the die
- Sheet of washed rubber dam increases friction & aids removal.
- Right hand fingers hold pattern & left hand die die pulled from pattern by
bending fingers of left hand. 52
53. J.WARPAGE OF WAX PATTERNS
- High tendency to warp or distort .
- Directly related to time of storage and temperature .
- Residual stresses developed in the pattern is associated with forces used to
shape the wax originally .
53
54. SOLUTION
- Softening the wax uniformly by heating at 50 degrees for 15 min.
- Warmed carving instruments and a warmed die .
- Adding wax in small amounts .
LOWER STORAGE TEMPERATURE :
- If a wax pattern is allowed to stand uninvested for longer than 30 Min – Keep it
in a refrigerator – Distortion is less in lower temperature.
- It should be warmed to room temperature before investing .
54
55. 5. SPRUE FORMER
MOLD: A negative form in which an object is cast/shaped.
SPRUE: The mold channel through which molten metal flows into the mold.
(or)
A Sprue is a channel in a refractory investment through mold through which
molten metal flows.
SPRUED WAX PATTERN: Wax form consisting of the prosthesis pattern
with attached sprue network.
55
56. A) PURPOSE OF SPRUE FORMER:
Create a channel – elimination of wax during burnout.
Channel – ingress of molten alloy during casting.
Compensate for alloy shrinkage during soldification.
56
57. B) SELECTION OF SPRUE FORMER:
Strickland etal (1958) stated the importance of the type, shape, location &
direction other than the size of the sprue.
Selection of the diameter & length of sprue former depends on the type & size
of wax pattern, type of casting machine & type of flask or casting ring used.
57
59. - Perfectly cylindrical in shape& smooth surfaces.
-Influence the burn out technique
- Wax – Most common
Metal –Hollow metal sprue is more preferred .
-They hold less heat than a solid sprue , this avoids overheating.
- Filled with sticky wax.
Plastic
- Plastic sprues melt at a higher temperature than wax
- Thermal expansion of wax is around 5 times that of plastic 59
60. D) DIAMETER OF THE SPRUE FORMER
Diameter Same size as the thickest area of wax pattern.
Melt velocity is proportional to sprue diameter.
In conjunction with the pressure of the casting machine & density of the
molten metal, controls the rate & flow of the molten metal.
Larger diameter of the sprue Distortion.
Smaller diameter Solidify before the casting itself &
Localized Shrinkage Porosity.
Solution: Reservoir sprues are used to help overcome this problem.
Range : 10-18 gauge (2.6-1.0mm)
Atleast 1.7 mm unless the pattern is extremely small
2.5 mm – Crowns
Large inlays – 14 gauge & Small inlay -16 gauge 60
61. E. SPRUE POSITION
Prefer At the occlusal surface (or)
Proximal wall or just below a nonfunctional cusp minimize grinding
of occlusal anatomy & contact areas.
Ideal Area: Point of greatest bulk in the pattern to avoid distorting thin areas of
wax during attachment to the pattern & permit complete flow of alloy.
61
62. F. SPRUE ATTACHMENT
Asgar & Peyton (1959) Flaring should occur at Sprue/wax pattern junction.
Flared for High density alloys.
Often restricted for lower density alloys.
Best for the molten alloy to flow from thick section to surrounding thin areas
(margins) rather than reverse.
Provide smooth flowing entry of gold into the mold and less porosity in the
casting minimizes risk for Turbulence.
All attachments , must therefore be TRUMPETED or FILLETED to eliminate all
sharp corners , angles and instrument marks . 62
65. G. THE LENGTH OF THE SPRUE FORMER
- Should be long enough to properly position the pattern in the casting
ring within 6 mm of the end of the ring yet short enough so that the
molten alloy doesn’t solidify before it fills the mold .
( 6mm – Gypsum bonded investments & 3-4mm –Phosphate bonded )
- Average sprue length – Large inlay – 4-5mm
Small inlay – 3-4mm
- Short sprue – Moves the pattern more away from the end of the ring
The gases cannot be adequately vented
Porosity 65
66. Long sprues – Solidify before the mold –
shrinkage porosity .
WHY 6mm ?
Provides adequate bulk of investment to
withstand force of inrushing gold, yet still
allows gases to escape from the end of the
mold .
More than 6 mm –
The gold will solidify before the entrapped air
can escape , resulting in rounded margins ,
incomplete casting , or mold fracture . 66
67. H. SPRUE DIRECTION
Shd be directed away from any thin or delicate parts of pattern molten metal
may abrade or fracture investment in this area.
Shd not be attached at a right angle to a broad flat surface lead of Turbulence
within mold cavity & porosity.
67
68. Sprued at 45 degree angle to proximal area satisfactory casting.
- Should always be directed towards the margins Favor the fine margins of
the wax patterns .
68
69. I. RESERVOIR
The reservoir is placed approximately 1.5mm from the pattern .
- Diameter should be greater than the bulkiest portion of the sprue .
Function – Prevents localized shrinkage porosity .
- Because of the large mass of alloy and position in the heat centre of the ring ,
the reservoir will remain molten to furnish liquid alloy into the Mold as it
solidifies .
- Resulting shrinkage will occur in the reservoir bar rather than the restorations.
69
71. J. CRUCIBLE FORMER
Funnel shaped.
Rubber, metallic or plastic.
Connected to sprue in same was as sprue attached to mold.
Wax pattern with sprue former is attached to crucible former in a special
locking area.
71
72. SPRUING
DIRECT SPRUING
The sprue former provides a direct connection between the pattern area and
the sprue base/ crucible former.
When two thick portions of wax are separated by thin wax, then 2 separate
sprues should be attached using direct spruing.
72
74. INDIRECT SPRUING
Indirect spruing uses the same basic principles of spruing. But the only difference
lies in attachment of 3 running horizontal bars. The whole indirect sprue
complex consist of 3 parts:
Manifold sprue.
Horizontal running bar.
Feeder sprue.
74
75. 6. CASTING RING
-Investment material is poured in the casting
ring & allowed to set around wax pattern.
CHOICE OF THE RING:
Rubber ring for HSE
Metal ring for TE
75
76. RING LESS CASTING SYSTEM
-Ringless Casting System is designed to increase productivity by achieving
consistently accurate results without the time-consuming steps associated with
the use of metal casting rings.
-Utilizes durable, reusable plastic rings that are tapered allowing for unimpeded
expansion of investment and easy removal of mold prior to burnout.
-This allows for quick and easy divesting after casting while reducing clean-up
chores.
-Investment expansion is easier to control and not limited to the thickness of a
ring liner.
76
78. CASTING RING LINERS
- The most commonly used technique to provide room for investment expansion.
Triple fold function :
- Freedom to expand which would otherwise be restricted by the ring .
- Helps to offset the contraction of the more rapidly cooling ring while the gold
alloy is being melted .
- In a wet liner certain amount of hygroscopic expansion is afforded
78
79. Traditionally – Asbestos ring liners
- Carcinogenic , biohazard .
NON ASBESTOS RING LINERS :
- Aluminium silicate ceramic liners – Can retain water on the surface .
- Cellulose ( paper ) liners – Better water absorption
Disadvantages: Burned away during casting , Difficult to secure in place.
- Absorb materials much less than asbestos , and their
combination with some gypsum bonded investments will produce fins
- Not compatible with phosphate bonded investments.
-Slightly higher expansion than asbestos liners.
79
80. Implications : Liner affords greater expansion in the investment
- Absorbed water causes a semihygroscopic expansion
as it is drawn into the investment
80
81. - The use of 1 liner increases the normal setting expansion compared with no
liner.
- A thicker liner provides even greater semi hygroscopic expansion and
also afford more unrestricted normal setting expansion .
LENGTH OF THE LINER :
Two concepts –
When maximum expansion is required – Flush with the open end
Smaller casting 3-6 mm (avg. 3.25mm) short of the end
1. Lock for the liner 2 . Uniform expansion
81
82. MANIPULATION OF A CASTING RING LINER
-Cut the liner to fit the inside diameter of the casting ring , no over lap.
- Dry liner technique – Dry liner is tacked in position with sticky wax .
-Wet liner technique –Lined ring is immersed in water and excess water is shaken
away . ( Squeezing-uneven water removal and expansion )
- Avoid touching or adapting with fingers reduce the cushioning effect.
- Attach the liner firmly to the ring by wax to prevent it from “riding up” during
investing and inadvertently affecting the size of the casting .
82
84. A. WETTING AGENTS or DEBUBBLIZERS
– Wax surfaces are not easily wetted by water
-If not covered by investment will develop surface irregularities in casting .
- Wettax- mild soap solution.
-These agents reduce the surface tension of the wax pattern , promotes better
wetting of the surface .
84
85. These agents decrease the contact angle of the liquid with the wax
surface.
Fig1 : 98degrees – untreated surface
Fig2 : 61degrees – treated surface more affinity for water
- investment being wetted with more ease
Fig3 : 91degrees –Rinsed with tap water and blotted dry
85
86. MANIPULATION
- Paint the debublizing solution on the pattern .
- Gentle air dry
- Don’t soak or rinse in water
- Don’t allow pooling in internal line angles of the pattern .
86
87. B. INVESTMENT MATERIALS
- A heat resistant or a refractory material used to form a
mold into which a metal or alloy is cast .
(OR) A molding material that surrounds the pattern & subsequently
hardens & forms the mold after the wax pattern is eliminated.
-The operation of forming the mold is called Investing .
Types – Gypsum bonded investments
Phosphate bonded investments
Ethyl silicate bonded investments
87
88. C. REQUIREMENTS OF AN IDEAL INVESTMENT MATERIAL:
Easily manipulated.
Sufficient strength at room temperature.
Stability at higher temperature
Sufficient expansion
Beneficial casting temperatures
Porosity
Smooth surface
Ease of divestment
Inexpensive.
88
91. BINDER: 30 to 35 %
Alpha hemihydrate form of gypsum OR Dental Stone.
MODIFIERS: 5%
Silica- Counterbalances gypsum shrinkage .
Chlorides – Reduces shrinkage below 700C
Sodium , Potassium , Lithium chlorides
BORIC ACID – Disintegrates during heating – Roughened Casting
91
92. ii) CLASSIFICATION:
Acc. To ADA Sp.no: 2- Casting Investments for dental gold alloys.
TYPE I – Inlays & Crowns Thermal expansion
TYPEII – Inlays & Crowns Hygroscopic expansion
TYPE III – Partial dentures with gold alloys.
Can withstand temperature upto 700 degrees C.
92
93. iii) SETTING TIME:
Not <5mins & not > 25mins.
Modern inlay investments set initially in 9 to 18 mins.
iv) SETTING EXPANSION:
PURPOSE: Aid in enlarging the mold to compensate partially for the casting
shrinkage .
3 Types: 1. Normal Setting Expansion
2. Hygroscopic Setting Expansion
3. Thermal Expansion.
93
94. 1. NORMAL SETTING EXPANSION-
- A mixture of silica and calcinated gypsum (calcium sulphate hemihydrate)
results in setting expansion greater than that of the gypsum product used
alone.
- Silica particles probably interfere with the intermeshing and interlocking of the
cystals as they form thrust of the crystals is outward during growth
increase expansion.
ANSI / ADA Specification No.2 for Type I investment permits a maximum
setting expansion in air of only 0.6%.
Setting expansion of such modern inlay investments is approx 0.4%.
It can be regulated by retarders and accelerators.
94
96. 2. HYGROSCOPIC EXPANSION
When gypsum products are allowed to set in contact with water, it leads to
outward growth of crystals expansion which is greater in magnitude than
normal setting expansion.
ANSI / ADA Specification No.2 for Type II investments requires
Minimum setting expansion in water of 1.2%;
Maximum expansion permitted is 2.2%.
96
98. FACTORS AFECTING HSE
Effect of composition
Effect of W:P Ratio
Effect of Temperature
Effect of time of immersion
Effect of Spatulation
Effect of Shelf Life of Investment
Effect of Confinement
Effect of the Amount of Added water.
98
99. 3. THERMAL EXPANSION:
Achieved by placing the mould in a furnace not greater than 700° C.
ANSI / ADA Specification No.2 requires that the thermal expansion of
- Type II investments be between 0% and 0.6% at 500° C.
For Type I investments, which rely principally on thermal expansion for
compensation, the thermal expansion must not be less than 1% nor greater
than 1.6%.
99
100. FACTORS AFFECTING THERMAL EXPANSION:
Effect of W:P ratio
Effect of Chemical modifiers
v) STRENGTH:
- Compressive strength for the inlay investments should not be less than 2.4 MPa
when tested 2 hrs after setting.
100
101. vi) THERMAL STABILITY:
Gypsum bonded investments decompose above 1200°C.
CaSO4+ SiO2 → CaSiO3 + SO3
CaSO4 + 4C →CaS + 4CO3
CaSO4 + CaS → 4CaO + 4SO2
Effects can be minimized by ‘heat soaking’ the investment mold at the casting
temperature to allow the reaction to be completed before casting commences.
vii) POROSITY:
The more gypsum crystals that are present in the set investment, the less is the
porosity.
The more uniform the particle size, the greater its porosity.
101
103. E. PROPERTIES:
i) TYPES:
TYPE I – For inlays, crowns and other fixed restorations.
TYPE II- For partial dentures and other cast, removable restorations.
ii) COMPOSITION:
POWDER- Ammonium diacid phosphate (NH4 H2 PO4)
Silica – Refractory
Magnesium oxide- reacts with phosphate ions.
LIQUID- In the form of silica sol in water.
iii) SETTING REACTION:
NH4 H2 PO4 + MgO→ NH4 MgPO4 + H2O
103
104. iv) SETTING EXPANSION-
With use of full strength liquid, about 0.4% attained.
Hygroscopic technique 0.6%- 0.8% can be realized.
THERMAL EXPANSION-
About 0.8% can be attained with a 50:50 mixture of liquid and water.
1% to 1.2% Use of undiluted liquid.
104
105. v) ADVANTAGES:
Easy to handle without breaking before they are placed in a furnace for the wax
burnout process and strong enough withstand the impact and pressure of
centrifugally cast molten alloy.
Provide setting and thermal expansions high enough compensate for the
thermal contraction of cast metal prostheses or porcelain veneers during
cooling.
Ability to withstand the burnout process(~1 to 1.5 hrs)with temperatures that
reach 900°C, and they can withstand temperatures upto 1000° C for short
periods of time.
105
106. vi) DISADVANTAGES :
When used with higher melting alloys, those with casting temperatures greater
than about 1,375° C, coupled with high mold temperatures result in mold
breakdown and rougher surfaces on castings.
High strength of these investments can make divesting ( removal of the casting
from the investment) a difficult and tedious process.
When higher expansion is required, more silica liquid is used results more
dense and less porous mold incomplete castings if a release for trapped gases
is not provided.
106
108. F. PROPERTIES:
- Silica is the binder.
SETTING EXPANSION (linear)-
Setting contractions of 0-0.4 %.
THERMAL EXPANSION-
- 1.5% to 1.8% can be attained between room temperature and 1000°C to 1177° C.
108
109. ADVANTAGES :
Cast high temperature cobalt- chromium and nickel-chromium alloys.
Good surface finishes, low distortion and high thermal expansion (good fit).
Thin sections with fine detail.
109
110. DISADVANTAGES:
Added processing attention and the extra precaution needed in handling the
low strength fired molds.
The low strength and high thermal expansion require a more precise burnout
process and firing schedule to avoid cracking and hence, destruction of a mold.
110
111. G. PREPARATION OF THE INVESTMENT MIX
Mixing of the investment is done by:
Hand mixing
Vacuum mixing
111
112. HAND INVESTING
- Water is added first slow addition of powder to remove air from powder.
-Hand spatulate the mix to incorporate the powder quickly.
- Cover of the bowlmechanical mixer mixed by hand.
- Coat the wax pattern with the investment
- Carefully coat the internal surface & the margin of the pattern
112
113. -Fill the ring slowly, starting from the bottom .
-Ring completely filled- leveled with top by edge of plaster spatula.
-Phosphate bonded investment – slightly overfilled – top is not levelled off.
-Investment set 45 to 60 min.
113
114. VACUUM INVESTING
-First hand spatulate the mix
-Attach the vacuum hose & mix
accordingly to the manufacturers
recommendations
-Invert the bowl & fill the ring under
vibration
-Remove the vacuum hose before setting
of the mixer
- Immediately clean the bowl & mixing
blade under running water
METHOD
114
115. H.SETTING OF INVESTMENT
It can be:
-In open air
-Hygroscopic technique
-Controlled water added technique
115
116. IN OPEN AIR
- Usually when High Heat TE technique is used.
- The investment is allowed to set in open air for 1 hour.
- The setting time is 1 hour for both GBI & PBI.
116
117. HYGROSCOPIC TECHNIQUE
- Once the casting ring is poured it is immersed into a water bath at 38 degrees
temperature immediately.
- This can be altered by:
-W:P ratio W:P HSE
-Time of immersion the delay HSE
-temp. of water HSE
117
118. CONTROLLED WATER ADDED TECHNIQUE
- The desired amount of expansion is retained by the amount of water added.
- A soft flexible rubber ring is employed & invested normally.
- A specific amount of water is added on the top of investment & allowed to set at
room temperature.
118
119. 8. WAX ELIMINATION OR BURN OUT
Elimination of the wax pattern from the mold of set investment material.
Investment set min. 1 hr.
Ideally kept in oven when mold is wet.
Delayed for several hours kept in humidor.
Rubber crucible former removed.
Place the sprue hole down at first , for easy draining out of wax Eliminated as
a liquid .
Invert ring , for the oxygen in the oven atmosphere to circulate more readily ,
to form gases rather than fine carbon which may interfere with venting .
119
121. IDEAL TEMPERATURE RANGES
- 500 degrees for one hour . ( Craig )
-Gypsum bonded investments -468degrees for hygroscopic technique 20mins
650degrees for thermal expansion
(or)
-Slow heating to 650-700 degrees in 60 minutes and held for 15 to 30 minutes at
the upper temperature .
-Phosphate bonded investments – Room temp. to max. 700 to 1030 degrees C
depending on alloy used for 30 mins.
315°C rapid heating held at the upper temperatures for 30 mins.
- General rule – Add 5 minutes to the wax elimination for every extra ring
placed in the oven at 500degrees C.
121
122. HYGROSCOPIC LOW HEAT TECHNIQUE
Sources of compensation expansion
• 37degree water bath
• Hygroscopic expansion by the warm water .
• Thermal expansion in the oven
ADVANTAGES :
- Less mold degradation
- Cooler surface for smoother castings
- Direct placement at 500 degrees – Large laboratories , time factor .
122
123. HIGH HEAT THERMAL EXPANSION
Compensation expansion factor – Thermal expansion produced by the high heat
burn out .
Accessory expansion factors :
- Setting of gypsum products .
- Water entering the wax pattern from liners and hence small amount of
Hygroscopic expansion .
123
124. TIME ALLOWABLE FOR CASTING
Investment contracts thermally as it cools.
When thermal expansion / high heat technique Investment loses
heat after heated ring removed from furnace and mold contracts.
124
125. 9. CASTING CRUCIBLES
3 types of casting crucibles are available : Clay, Carbon and Quartz (Zircon
alumina).
Clay crucible are – many of crown bridge alloys such as high noble-alloy.
Carbon crucible high noble crown bridge , higher fusing , gold based metal
ceramic.
Quartz crucibles High fusing alloys of any type suited for alloys that have a
high melting range and are sensitive to carbon contamination.
Palladium silver from metal ceramic copings.
Nickel/cobalt based alloys.
125
129. 10. METHODS OF MELTING THE ALLOY
METHODS :
TORCH ELECTRICAL
Gas/Air (Most Common) Resistance
Gas/Oxygen – PFM,Pd Induction
Air /Acetylene Direct Current Arc
Oxygen /Acetylene
129
130. TORCH MELTING
- The alloy is melted in a separate crucible by a torch flame and is cast into the
mold by centrifugal force.
-Temperature of gas-air flame is influenced by
i) Nature of the gas &
ii) Proportion of gas and air in the mixture.
-Considerable care Obtain a non-luminous brush flame, with combustion
zones clearly differentiated for melting the alloy .
130
131. ZONES OF A FLAME
Zone 1 – Directly from the nozzle
Air and gas are mixed before combustion .
No heat is present
Zone 2 – Combustion zone
Gas & Air are partially burned
Color – GREEN
Oxidizing – KEEP AWAY 131
132. Zone 3 : Reducing zone
Hottest part of the flame.
Most effective zone for melting and should be kept constantly over the alloy .
Color – Blue
Zone 4 : Oxidizing zone
Combustion occurs with the oxygen in the air .
KEEP AWAY .
132
133. CRAIG’S METHOD FOR DETERMINING THE EFFECTIVE FLAME :
-Checking & interpreting the flame condition.
Apply the flame to a copper coin – on a soldering block.
Bright & Clean Dark , dull red colour
Oxidation and ineffective heating
Visual scenario practically : Morphology
Spongy Small globules of fused metal appear Spheroidal shape
Color :
- The molten alloy is light orange and tends to spin or follow the flame when it
is moved slightly. 133
135. Disadvantages :
Excessive heat may distill lower melting components .
Overheating – gases to dissolve in the casting – porosity
Highly technique sensitive
AIR ACETYLENE & OXYGEN ACETYLENE GAS
- These were designed mainly for Cobalt chromium base alloys higher fusion
temperatures
Advantage : Hottest flame hence faster burnout .
135
136. ELECTRICAL RESISTANCE -- HEATED CASTING MACHINE
PRINCIPLE :
- During Electrical melting of alloys heat energy is produced when electric
current is passed through a conductor depending upon the voltage applied
across it.
- The alloy is melted electrically by a resistance heating .
- Current is passed through a resistance heating conductor, and automatic
melting of the alloy occurs in a graphite or ceramic crucible.
136
137. - Resistance heat develops when flow of current was opposed by a opposite power
e p
e
pe
p
e
p
RESISTANCE HEATING
137
138. Advantages:
For metal ceramic prosthesis.
Base metals in trace amounts that tend to oxidize on overheating.
Crucible located flush against casting ring.
Carbon crucibles should not be used in melting of:
High Pd
Pd-Ag
Ni-Cr
Co-Cr
138
140. INDUCTION MELTING MACHINE
The alloy is melted by an induction field that develops within a crucible
surrounded by water-cooled metal tubing.
140
143. The electric induction furnace is a transformer in which an alternating current
flows through the primary winding coil and generates a variable magnetic field
in the location of the alloy to be melted in a crucible
143
144. Alloy reaches melting temp. forced into mold by air pressure, or by
vacuum.
It is more commonly used for melting base metal alloys, more in
jewelry .
Not been used for noble alloy casting as much as other machines.
144
146. The temperature within the arc exceeds 4000oC and the alloy melts very quickly.
This method has a high risk for over heating the alloy.
146
147. - Casting machines provide the means for transferring the molten alloy from the
crucible to the mold
11. CASTING MACHINES
147
148. OBJECTIVES OF CASTING
1) Alloy should be heated as qucikly as possible to a completely molten condition
(above liquidus temp.)
2) Oxidation of alloy prevented heating metal with a well adjusted torch &
small amount of flux on metal surface.
3) Adequate force applied to force the well-melted metal into the mold.
148
149. 149
TYPES
CENTRIFUGAL CASTING MACHINE:
The alloy is melted in separate crucible by a torch flame and the metal is cast into
the mold by centrifugal force.
HIGH FREQUENCY CENTRIFUGAL CASTING MACHINE:
The alloy is melted electrically by a resistance or induction furnace, then cast into
the mold centrifugally by motor or spring action.
VACUUM OR PRESSURE ASSISTED CASTING MACHINE:
The alloy is melted by a torch flame or electrically and then cast into mold by air
pressure and / or by vacuum.
150. .
Acc. To William J. O’ Brien:
1. Centrifugal force type
2. Pneumatic force (or) Air pressure type.
150
151. CASTING TECHNIQUES
CENTRIFUGAL FORCE TYPE PNEUMATIC FORCE
Spring loaded
torch melting
machine
Induction melting
machine
Electrical
resistance heated
casting machine
Electric arc vacuum
casting machine
151
152. ACCORDING TO SH SORATUR
1. Centrifugal casting machine
2. Steam Pressure machine-Solbrig machine
3. Air pressure machine – Hereus
4. Spring wound Electrical resistance-melting furnace-casting
machine
5. Induction melting casting machine
152
153. VACUUM OR PRESSURE ASSISTED CASTING MACHINE
1ST evacuate the melting chamber to reduce oxidation.
Apply air pressure uniformly about the casting ring forcing molten alloy into
mold.
Vacuum is applied to the bottom of the mold.
Molten alloy is “PUSHED & SUCKED” into the mold by gravity or vacuum.
Used for titanium and titanium alloys.
153
156. CENTRIFUGAL CASTING MACHINE
This machine utilize the centrifugal force which is defined as a radial force
radiating outward from the center of rotation of a body, for casting.
156
158. - The machine works on ‘broken-arm’ principle crucible is attached to the
broken-arm, which accelerates the effective initial rotational speed of the
crucible and casting ring thus increasing the linear speed of the liquid casting
alloy as it moves into and through the mold.
- To counter the weight of the molten metal in the crucible and casting ring,
balancing arm is provided with the balancing weights.
158
159. The casting machine is given three (or) four clock wise turns and locked in
position with the pin.
159
160. A claycarbon crucible for the gold alloy being cast is placed in the machine.
The torch is lit and adjusted.
160
161. This preheating avoids excessive slag formation during casting.
PREHEATING CRUCIBLE
161
162. - Alloy is placed on the inner sidewall of the crucible heated in the reducing
part of the flame until it is ready to cast.
- Properly adjusted torch develops adequate temp. 870-1000 degrees C.
-Alloy should be approx. 38°C to 66°C above liquidus temperature.
-The casting should be made when proper temperature is reached
- No more 30 secs should be allowed to elapse between the time the ring is
removed from the oven and the molten alloy is centrifuged into the mold.
- When the alloy is molten,slide the crucible against the ring, sprinkle flux over
the metal.
162
164. A reducing flux is used in melting the alloy (50% boric acid powder and 50%
fused borax ) it increases fluidity and reduces potential for oxidation.
164
165. When reducing zone is in contact-the surface of the gold is bright and mirror
like.
Oxidizing zone in contact-dull film or “dross” development.
When gold alloy is ready to cast it will be white hot, forming smooth pool.
165
166. Hold the casting arm so that the
pin drops away
Release the arm and rotate till it
comes to rest
Providing enough force to cause
the liquid alloy to flow into the
mold.
-
166
167. •Once the metal fills the mold there is a hydrostatic pressure gradient developed
along the length of the casting.
• The pressure gradient from the tip of the casting(0.21 to 0.28 Mpa/ 30 to 40 psi)
to the button surface is quite sharp and parabolic in function, coming to zero at
the button surface.
•Because of this gradient there is also a gradient in the heat transfer rate, such
that the greatest rate of heat transfer to the mold is at the high pressure end of the
gradient (i.e. the tip of the casting).
•Therefore, solidification progresses from tip to the button side.
•The arm should be stopped with brake lever only when it gets slowed down
naturally and the ring is removed with casting tongs.
167
169. QUENCHING
After the casting has solidified, the ring is removed and quenched in water as
soon as the button exhibits a dull-red glow.
Ring is quenched sprue open & button upwards 2/3rd length of ring is
dipped in water.
169
170. ADVANTAGES OF QUENCHING
1.Upward direction of sprue compensates casting shrinkage.
2. Metal alloy left in an annealed condition for burnishing, polishing,..
3. When water contacts the hot investment easy removal & soft granular
investment.
170
171. DIVESTING
Removal of Investment / Recovery of Casting.
End of the ring for about ¼ inch
Bulk – finger pressure.
- Sprue is removed from the restoration using an carborundum
separating disk/ abrasive disk mounted in a hand piece.
171
174. PICKLING
- Removal of oxide residues of carbon by heating the discoloured casting in an
acid.
- SOLUTIONS USED: 50% HCL, PHOSPHORIC ACID, HYDROFLUORIC ACID
-Advantages of HCl:
Aids in removal of residual investment as well as oxide coating
-Disadvantages:
Likely to corrode laboratory metal furnishings
Fumes are health hazard
-Method of cleaning :
Place the casting in test tube or dish and pour acid over it
- Other methods: Heating the casting and then dropping into the pickling
solution
174
176. SAND BLASTING
Casting is held in an sand blasting machine to
clean the investment from the surface.
The blasting materials used are:
Sand shells
Recycled Aluminium oxide with pressure of
100psi
Garnet
Ultrasonic cleaners
Abrasive spray devices
176
177. Finishing and polishing : Brown or White Al2O3 stones are used.
177
- Rag or felt wheels impregnated with abrasives are used in the initial phase of this
stage.
- Final polishing is achieved using various oxides of tin and aluminium used in
conjunction with a small rag or chamois buffing wheel, followed with an iron
oxide rouge.
- Residual traces of rosin or waxlike matrix from oxides Polishing compound
remover followed by a hot, soapy water rinse.
178.
179. CAUSES OF CASTING DEFECTS
ACCORDING TO PHILLIP’S
1. DISTORTION
2. SURFACE ROUGHNESS, IRREGULARITIES, DISCOLORATION
1. a. Air bubbles
2. b. Water film
3. c. Rapid heating
4. d. Under heating
5. e. L/P ratio.
6. f. Prolonged heating
7. g.Temperature of alloy
8. h.Casting pressure
9. i.Composition of investment
10. j. Foreign bodies
11. k. Impact of molten alloy
12. l. Pattern position
13. m. Carbon inclusions 179
180. 3. POROSITY
I. Solidification defects
A. Localized shrinkage porosity
B. Microporosity
II. Trapped gases
A. Pinhole porosity
B. Gas inclusions
C. Subsurface porosity
III. Residual air
4. INCOMPLETE CASTING
180
181. An unsuccessful casting results in considerable trouble and loss of time.
Defects in castings can be avoided by strict observance of procedures governed
by certain fundamental rules and principles.
181
182. ACCORDING TO O’BRIEN CASTING PROBLEMS CAN BE
CLASSIFIED :
A. GENERAL PROBLEMS
1. Problems with accuracy
2. Problems with distortion
3. Problems with bubbles
4. Problems with surface roughness
5. Problems with fins on the surface or margins
6. Problems with short and rounded margins
7. Problems with miscasting
8. Problems with pits 182
183. B. PROBLEMS WITH INTERNAL POROSITY
9. Problems with localized shrinkage porosity
10. Problems with subsurface porosity
11. Problems with microporosity
C. PROBLEMS WITH EXTERNAL POROSITY
12. Problems with back pressure porosity
183
184. 1. DISTORTION
Any marked distortion of the casting is related to distortion of the wax pattern
Setting and hygroscopic expansions of the investment may produce a
nonuniform expansion of the walls of the pattern.
The gingival margins are forced apart by the mold expansion, whereas the solid
occlusal bar of wax resists expansion during the early stages of setting.
184
185. Configuration of the pattern, the type of wax, and the thickness influence the
distortion.
Distortion increases as the thickness of the pattern decreases
Less the setting expansion of investment less the distortion
STUDY: Cast post made with an unlined metal casting ring may exhibit
anisotropic shrinkage which could result in distortion.
185
186. Wax too hot- Excessive shrinkage results on cooling.
Wax too cool- The pattern undergoes stress release with change in shape.
Insufficient pressure during waxing- The pattern distorts because of
thermal shrinkage.
Delayed investment- The sooner the investment is complete, the less
distortion
Heating pattern during spruing- Create distortion.
Overheating casting during soldering procedure- This warps or melts the
margins.
186
187. TO AVOID DISTORTION
Appropriate selection of investing material with less setting expansion
Invest the wax pattern as early as possible
Proper handling of the wax pattern
187
188. 2. SURFACE ROUGHNESS, IRREGULARITIES, AND
DISCOLORATION
The surface of a dental casting should be an accurate reproduction of the
surface of the wax pattern from which it is made.
Excessive roughness or irregularities on the outer surface of the casting
necessitate additional finishing and polishing.
188
189. SURFACE ROUGHNESS
DEFINED: Relatively finely spaced surface imperfections whose height, width,
and direction establish the predominant surface pattern.
PROBLEMS WITH SURFACE ROUGHNESS
Water/powder ratio- A high ratio increases the roughness of the mold.
Excess wetting agent or salivary contamination - This may form a film on
the pattern surface and be reproduced on the casting surface.
Prolonged heating or overheating of the mold - may cause investment
disintegration, Roughness appears general and feels sharp.
Premature heating of casting investment- Wait a minimum of 45 minutes
for burnout.
189
190. SURFACE IRREGULARITIES
Surface irregularities are isolated imperfections, such as
nodules, that are not characteristic of the entire surface area.
Irregularities on the cavity surface prevent a proper seating of
an otherwise accurate casting.
190
191. a) AIR BUBBLES:
Small nodules on a casting are caused by air bubbles that become attached
to the pattern during or subsequent to the investing procedure.
Nodules can sometimes be removed not in a critical area.
Nodules on margins or on internal surfaces removal of these
irregularities might alter fit of the casting
192
192. Inadequate vacuum or ineffective painting procedure- Vacuum must have
at least 26mm mercury for vacuum investing.
Water/powder ratio - Investment is too thick, it will not cover the pattern
completely.
Excessive vibration of the ring- Produces small nodules.
NODULES
193
194. TO AVOID AIR BUBBLES
Proper mixing of the investment if manual method is used
Use of a mechanical mixer with vibration both before and after mixing
Vaccum investing technique is the best method.
Use of a wetting agent in a thin layer
195
195. b) WATER FILMS:
Wax is repellent to water and if the investment becomes separated from the
wax pattern in some manner, a water film may form irregularly over the surface.
Appears as minute ridges or veins on the surface.
Too high L/P ratios .
Pattern is slightly moved, or vibrated after investing or if the painting procedure
does not result in an intimate contact of the investment with the wax pattern .
196
196. TO AVOID WATER FILMS
Use of a wetting agent in a thin layer
Using Correct water - powder ratio
197
197. c) RAPID HEATING
Result in formation of fins or spines on the surface of the casting
Due to the flaking of the investment when water or steam pours into the mold
A surge of steam or water may carry certain salts into the mold that are left
behind in the walls as the water evaporates
198
198. FINS ON THE SURFACE OR MARGIN - DUE TO
Prolonged heating- Cracks in the investment that radiate out from the
surface of the pattern.
Heating rate is too rapid- Cracks may appear in the investment, caused by
nonuniform heating of investment.
Water/powder ratio- A high ratio produces a weak investment that may
crack.
Excessive casting pressure- Metal impact may cause investment fracture.
Cooling of the investment prior to casting- Cracks in the investment
199
199. TO AVOID FINS OR SPINES
Gradual heating of the mold- atleast 60 min should elapse during the heating
of the investment- filled ring from room temperature to 700º C.
Greater the bulk of the investment, more slowly it should be heated.
200
200. d) UNDERHEATING
Incomplete elimination of wax residues may occur if the heating time is too
short or if insufficient air is available in the furnace.
Low-temperature investment techniques
Voids or porosity may occur in the casting from the gases formed when the hot
alloy comes in contact with the carbon residues.
Casting may be covered with a tenacious carbon coating that is virtually
impossible to remove by pickling
201
201. e)LIQUID/POWDER RATIO
The amount of water and investment should be measured accurately.
The higher the L/P ratio, the rougher the casting.
Too little water Investment thick and cannot be properly applied to the
pattern.
In vacuum investing, the air may not be sufficiently removed.
TO AVOID
Use the correct W/P ratio according to manufacturer’s instructions.
202
202. F)PROLONGED HEATING
High-heat casting technique a prolonged heating of mold at the casting
temperature disintegration of the gypsum-bonded investment, and the walls
of the mold are roughened.
Products of decomposition are sulfur compounds that may contaminate the
alloy to the extent that the surface texture is affected.
TO AVOID
Thermal expansion technique is employed mold heated to the casting
temperature and never higher.
The casting should be made immediately.
203
203. g) TEMPERATURE OF THE ALLOY
Alloy is heated to too high a temperature before casting, the surface of the
investment is likely to be attacked, and a surface roughness may result.
In all probability, the alloy will not be overheated with a gas-air torch when
used with the gas supplied in most localities.
If other fuel is used, special care should be observed that the color emitted by
the molten gold alloy, for example, is no lighter than a light orange.
204
204. h) CASTING PRESSURE
Too high a pressure during casting can produce a rough surface on the casting
TO AVOID
a gauge pressure of 0.10 to 0.14 MPa in an air pressure casting machine (or)
3 to 4 turns of spring in an average type of centrifugal casting machine is
sufficient for small castings.
205
205. i) COMPOSITION OF THE INVESTMENT
The ratio of the binder to the quartz influences the surface texture of the
casting.
A coarse silica causes a surface roughness.
If the investment meets ANSI/ADA specification n0.2, the composition is
not a factor for surface roughness
206
206. j) FOREIGN BODIES
When foreign substances get into the mold, a surface roughness may be
produced.
Rough crucible former with investment clinging bits of investment are
carried into the mold with the molten alloy
Carelessness in the removal of the sprue former
Sharp, well-defined deficiencies pieces of investment and bits of carbon
from a flux.
207
207. Bright-appearing concavities Flux being carried into the mold with the
metal.
Surface discoloration and roughness can result from sulfur contamination
The interaction of the molten alloy with sulfur produces a black or grey layer on
the surface of gold alloys that is brittle and does not clean readily during
pickling.
208
208. K) IMPACT OF MOLTEN ALLOY
Direction of sprue former molten gold alloy does not strike a weak portion
of the mold surface.
Molten alloy may fracture or abrade the mold surface on impact, regardless of
its bulk.
TO AVOID
Proper Spruing To prevent the impact of molten metal at an angle of
90 degrees to investment surface.
209
209. l) PATTERN POSITION
If several patterns are invested in the same ring, it causes breakdown or
cracking of the investment if the spacing between the patterns are less than
3mm.
B/c expansion of wax is much greater than that of the investment.
TO AVOID
Do not place several patterns too close together if invested in the same ring
Avoid too many patterns in the same plane in the mold
210
210. m) CARBON INCLUSIONS
Carbon, as from a crucible, an improperly adjusted torch, or a carbon-
containing investment, can be absorbed by the alloy during casting.
May lead to the formation of carbides or even create visible carbon inclusions.
211
211. 3. POROSITY
Porosity may occur both within the interior region of a casting and on the
external surface.
The latter is a factor in surface roughness, but also it is generally a manifestation
of internal porosity.
Not only does the internal porosity weaken the casting but if it also extends to
the surface, it may be a cause for discoloration.
If severe, it can cause plaque accumulation at the tooth-restoration interface,
and secondary caries may result.
Although the porosity in a casting cannot be prevented entirely, it can be
minimized by use of proper techniques. 212
212. POROSITIES IN METAL ALLOY CASTINGS MAY BE
CLASSIFIED AS FOLLOWS:
I. Solidification defects
A. Localized shrinkage porosity
B. Microporosity
II. Trapped gases
A. Pinhole porosity
B. Gas inclusions
C. Subsurface porosity
III. Residual air
213
213. LOCALIZED SHRINKAGE POROSITY
CAUSE: Premature termination of the
flow of molten metal during solidification.
Linear contraction of noble metal alloys in changing from a liquid to a
solid is at least 1.25%.
SOLUTION: Continual feeding of molten metal through the sprue
make up for the shrinkage of metal volume during solidification.
Generally occurs : Near the sprue-casting junction
Alloy or mold temperature is too low -Rapid solidification of the alloy
214
214. TO AVOID LOCALIZED SHRINKAGE POROSITY
Using sprue of appropriate thickness
Attach the sprue to the thickest portion of the wax pattern
Flare the sprue at the point of attachment or placing a reservoir close to the wax
pattern
215
215. HOT SPOT: The entering metal impinges onto the mold surface at a point
and creates a higher localized mold temperature.
A hot spot may retain a localized pool of molten metal after other areas of the
casting have solidified.
This in turn creates a shrinkage void, or suck-back porosity.
216
216. SUCK -BACK POROSITY: Hot spot causes the local region to freeze last
and results suck-back porosity.
Suck-back porosity often occurs at an occlusoaxial line angle or incisoaxial line
angle that is not well rounded.
217
217. TO AVOID SUCK BACK POROSITY
Flare the sprue at the point of attachment to the wax pattern
Reduce the mold – melt temperature differential, that is lowering the casting
temperature by about 30ºC.
With a higher mold temperature, the difference in temperature between the
investment located around the sprue and the investment in the area of the
pulpal floor of the full crown is decreased.
This decrease helps the molten alloy at the pulpal floor to solidify before the
alloy at the sprue
218
218. MICROPOROSITY
Occurs from solidification shrinkage but is generally present in fine-grain alloy
castings when the solidification is too rapid for the microvoids to segregate to
the liquid pool.
This premature solidification causes the porosity in the form of small, irregular
voids.
Such phenomena can occur from rapid solidification if the mold or casting
temperature is too low.
219
219. PINHOLE AND GAS INCLUSION POROSITIES
Related to the entrapment of gas during solidification.
Both Spherical contourdifferent in size.
The gas inclusion porosities are usually much larger than pinhole porosity.
220
221. Many metals dissolve or occlude gases while they are molten.
On solidification, the absorbed gases are expelled and pinhole porosity results.
All castings certain amount of porosity
Porosity should be kept to a minimum adversely affect the physical
properties of the casting.
Porosity surface form of small pinpoint holes
Surface is polished, other pinholes appear.
Larger spherical porositiespoorly adjusted torch flame, or by use of the
mixing or oxidizing zones of the flame.
222
222. SUBSURFACE POROSITY
Simultaneous nucleation of solid grains and gas bubbles
at the first moment that the alloy freezes at the mold walls.
Short, thick sprue pin- Rapid entry of the alloy causes skin formation; the
bulk of alloy pulls away, forming subsurface porosity.
Alloy or mold temperature is too high - The first portion of gold to contact
the investment will solidify and form a thin skin. The alloy behind it shrinks
during solidification and pulls away, forming small porosities.
Controlled Rate of molten metal that enters the mold
223
223. ENTRAPPED-AIR POROSITY
- Occurs on the inner surface of the casting, sometimes referred to as
BACK-PRESSURE POROSITY large concave depressions
Caused by the inability of the air in the mold to escape through the pores in the
investment or by the pressure gradient that displaces the air pocket toward the
end of the investment.
224
224. The incidence of entrapped increased by
- Use of the dense modern investments,
- By an increase in mold density produced by vacuum investing, and
- By the tendency for the mold to clog with residual carbon when the low-heat
technique is used.
Slow the venting of gases from the mold during casting.
225
225. According to William O Brien
Insufficient alloy mass- Air is entrapped in the solidifying alloy.
Insufficient turns on the casting machine - Denser the investment, the
greater the force needed to eliminate the gas within the mold chamber.
Pattern is too for away from the end of the ring - Dense investments and
lower burnout temperatures
226
226. TO AVOID ENTRAPPED AIR POROSITY
Proper burnout
Adequate mold and casting temperature
High casting pressure
Proper L/P ratio
Thickness of the investment between the tip of the pattern and the end of the
ring not greater than 6mm.
227
227. 4. INCOMPLETE CASTING
Partially complete casting, or perhaps no casting at all, is found.
The obvious cause is that the molten alloy has been prevented, in some manner,
from completely filling the mold.
Two factors that may inhibit the ingress of the liquefied alloy are
- Insufficient venting of the mold and
- High viscosity of the fused metal.
228
229. Insufficient venting, is directly related to the back pressure exerted by the air in
the mold.
If the air cannot be vented quickly, the molten alloy does not fill the mold
before it solidifies.
In such a case, the magnitude of the casting pressure should be suspected.
If insufficient casting pressure is used, the back pressure cannot be overcome
230
230. Furthermore, the pressure should be applied for at least 4 sec.
The mold is filled and the alloy is solidified in 1 sec or less; yet it is quite soft
during the early stages.
Therefore the pressure should be maintained for a few seconds beyond this
point.
These failures are usually exemplified in rounded, incomplete margins.
ROUNDED, INCOMPLETE MARGINS
231
232. Second common cause for an incomplete casting is incomplete elimination of
wax residues from the mold.
If too many products of combustion remain in the mold, the pores in the
investment may become filled so that the air cannot be vented completely.
If moisture or particles of wax remain, the contact of the molten alloy with
these foreign substances produces an explosion that may produce sufficient
back pressure to prevent the mold from being filled.
233
233. According to William O Brien
Casting is nearly or entirely missing - The pattern detached from the sprue
pin, due to excessive vibration.
Pattern fractured during investing
Gold alloy was too cold during casting
Incomplete burnout
Sprue pin was too small - If the sprue freezes before the alloy fills the mold
completely, incomplete casting results.
234
234. CONCLUSION
Thus, these are the various causes for the failure of the castings and
methods by which these defects can be avoided, thereby
producing a casting of good quality for clinical success.
235
236. 6.NOTES ON DENTAL MATERIALS – VK SUBBARAO
7. SYNOPSIS OF DENTAL MATERIALS – S GOWRI SHANKAR
8. TEXT BOOK OF SCIENCE OF DENTAL MATERIALS
9. ESSENTIALS OF DENTAL MATERIALS - SH. SORATUR
10. PRINCIPLES & PRACTICE OF OPERATIVE DENTISTRY –
CHARBENEAU – 3RD EDITION.
237
237. 11. JOURNAL OF PROSTHETIC DENTISTRY-1987,57,362-368
12. JOURNAL OF PROSTHETIC DENTISTRY -1989,61,418-424
13. DENTAL MATERIALS JOURNAL -1993 DEC 12 (2) 245-52.
14. DENTAL MATERIALS JOURNAL-2009 MAY 25 (5) 629-33.