This document reports on a study that used differential scanning calorimetry (DSC) to characterize the thermal stability and phase transformation properties of four welding consumables developed for welding modified 9Cr-1Mo ferritic steel. DSC was used to precisely determine transformation temperatures like Ac1 and Ac3 as well as solidus and liquidus temperatures. The kinetics of austenite formation from tempered martensite was also modeled. It was found that Ac1 and Ac3 decreased with increasing (Mn+Ni) content and that apparent activation energy for austenite formation was sensitive to heating rate. An activation energy of around 260 kJ/mol was suggested for the α→γ transformation in high chromium steels
Welding Studies on WB36 for Feed Water Pipingijceronline
To increase efficiency, reduce emissions, cost and to reduce weight of boiler per MW, the power manufacturing sectors are going towards the once through technology (super critical boiler) instead of sub- critical. Once through supercritical (OTSC) technology has become a focal point for effective utilization of coal-based thermal power generation sector in India. Another main advantage of moving towards OTSC technology is reducing the weight of the boiler per MW, which can be done by going for material capable of handling higher pressure and temperature than the conventional material. So, in order to keep pace with these technologies, research on newer materials for every boilers line, which can operate at both higher pressure and temperature, has been initiated. So, in this article, we have taken one such feed water system and headers, where WB 36 steel (15 MiCuMoNiNb5) can be used instead conventional standard carbon steel like A106 grade B or C, which are usually used. For super critical, ultra super critical power plants this conventional materials like A106 grade B or C, leads to very thick piping system. V&M has developed WB 36 steel (15 MiCuMoNiNb5) for high pressure piping of boiler feed water system. This heat-resistant, copperalloyed ferritic steel 15MiCuMoNiNb5 has been widely used in European nuclear and conventional power plants for decades for feed water system. This widespread application is due to the toughness and strength, caused by the precipitation of copper, that are exhibited even at elevated temperatures which other fine-grained structural steels have at room temperature. The aim of this project “Welding Studies on WB36 Steel for Feed Water Piping” was taken to understand the metallurgy and the behavior of the new materials under different manufacturing operations.
International Journal of Engineering Research and DevelopmentIJERD Editor
Electrical, Electronics and Computer Engineering,
Information Engineering and Technology,
Mechanical, Industrial and Manufacturing Engineering,
Automation and Mechatronics Engineering,
Material and Chemical Engineering,
Civil and Architecture Engineering,
Biotechnology and Bio Engineering,
Environmental Engineering,
Petroleum and Mining Engineering,
Marine and Agriculture engineering,
Aerospace Engineering.
Development of dual phase steel and determination its of mechanical propertiesIAEME Publication
In this paper, the development of dual phase steel from low carbon steel and mechanical
properties have been studies. Dual phase steel is developed by intercritical annealing in order to
improve the hardness and impact toughness. Low carbon steel of 0.21% carbon content is first
intercritically heated in furnace and then rapid cooling in water is done to obtain the martensitic
steels. Different samples of DP steels are prepared by the intercritical annealing process temperature
ranging from740˚C to 840˚C. The heating temperature and different time of heating of the steel is
used to make different percentage of Maternsite steel. Dual phase steel so obtained is now tested and
properties of the DP steel are evaluated. Hardness, charpy, microstructure test for each specimen is
conducted to compare its hardness and toughness with low carbon steel. The mechanical properties
of heat treated and non heat treated specimens are obtained and compared. The result indicates that
the specimen hardness and toughness are proportional to amount of martensite and amount of
martensite depends on intercritical annealing temperature.
International Journal of Engineering and Science Invention (IJESI) is an international journal intended for professionals and researchers in all fields of computer science and electronics. IJESI publishes research articles and reviews within the whole field Engineering Science and Technology, new teaching methods, assessment, validation and the impact of new technologies and it will continue to provide information on the latest trends and developments in this ever-expanding subject. The publications of papers are selected through double peer reviewed to ensure originality, relevance, and readability. The articles published in our journal can be accessed online.
Magnetic nde characterization of tempered 2.25 cr 1mo steelAPOORVKRISHNA1
A descriptive presentation on heat treatment analysis of Tempered 2.25Cr-1Mo steel ,commonly known as P22 steel. The presentation includes history of the material, objective and work-plan with procedures adopted to carry out the project.
Welding Studies on WB36 for Feed Water Pipingijceronline
To increase efficiency, reduce emissions, cost and to reduce weight of boiler per MW, the power manufacturing sectors are going towards the once through technology (super critical boiler) instead of sub- critical. Once through supercritical (OTSC) technology has become a focal point for effective utilization of coal-based thermal power generation sector in India. Another main advantage of moving towards OTSC technology is reducing the weight of the boiler per MW, which can be done by going for material capable of handling higher pressure and temperature than the conventional material. So, in order to keep pace with these technologies, research on newer materials for every boilers line, which can operate at both higher pressure and temperature, has been initiated. So, in this article, we have taken one such feed water system and headers, where WB 36 steel (15 MiCuMoNiNb5) can be used instead conventional standard carbon steel like A106 grade B or C, which are usually used. For super critical, ultra super critical power plants this conventional materials like A106 grade B or C, leads to very thick piping system. V&M has developed WB 36 steel (15 MiCuMoNiNb5) for high pressure piping of boiler feed water system. This heat-resistant, copperalloyed ferritic steel 15MiCuMoNiNb5 has been widely used in European nuclear and conventional power plants for decades for feed water system. This widespread application is due to the toughness and strength, caused by the precipitation of copper, that are exhibited even at elevated temperatures which other fine-grained structural steels have at room temperature. The aim of this project “Welding Studies on WB36 Steel for Feed Water Piping” was taken to understand the metallurgy and the behavior of the new materials under different manufacturing operations.
International Journal of Engineering Research and DevelopmentIJERD Editor
Electrical, Electronics and Computer Engineering,
Information Engineering and Technology,
Mechanical, Industrial and Manufacturing Engineering,
Automation and Mechatronics Engineering,
Material and Chemical Engineering,
Civil and Architecture Engineering,
Biotechnology and Bio Engineering,
Environmental Engineering,
Petroleum and Mining Engineering,
Marine and Agriculture engineering,
Aerospace Engineering.
Development of dual phase steel and determination its of mechanical propertiesIAEME Publication
In this paper, the development of dual phase steel from low carbon steel and mechanical
properties have been studies. Dual phase steel is developed by intercritical annealing in order to
improve the hardness and impact toughness. Low carbon steel of 0.21% carbon content is first
intercritically heated in furnace and then rapid cooling in water is done to obtain the martensitic
steels. Different samples of DP steels are prepared by the intercritical annealing process temperature
ranging from740˚C to 840˚C. The heating temperature and different time of heating of the steel is
used to make different percentage of Maternsite steel. Dual phase steel so obtained is now tested and
properties of the DP steel are evaluated. Hardness, charpy, microstructure test for each specimen is
conducted to compare its hardness and toughness with low carbon steel. The mechanical properties
of heat treated and non heat treated specimens are obtained and compared. The result indicates that
the specimen hardness and toughness are proportional to amount of martensite and amount of
martensite depends on intercritical annealing temperature.
International Journal of Engineering and Science Invention (IJESI) is an international journal intended for professionals and researchers in all fields of computer science and electronics. IJESI publishes research articles and reviews within the whole field Engineering Science and Technology, new teaching methods, assessment, validation and the impact of new technologies and it will continue to provide information on the latest trends and developments in this ever-expanding subject. The publications of papers are selected through double peer reviewed to ensure originality, relevance, and readability. The articles published in our journal can be accessed online.
Magnetic nde characterization of tempered 2.25 cr 1mo steelAPOORVKRISHNA1
A descriptive presentation on heat treatment analysis of Tempered 2.25Cr-1Mo steel ,commonly known as P22 steel. The presentation includes history of the material, objective and work-plan with procedures adopted to carry out the project.
Remaining life assessment of refinery furnace tubes using finite element methodBarhm Mohamad
Crude oil heater 9Cre-1Mo steel tubes from a refinery plant were studied, after 5 years of service at nominally 650 Cº and 3 bar, to predict their remnant lives. The investigation included dimensional, hardness and tensile measurements in addition to accelerated stress rupture tests between 650 Cº and 700 Cº and microstructural examination. Tube specimens were taken from two sections, the overheated side and the side which only saw the nominal operating temperature. The method employed involved the prediction of the increase in temperature with increasing sediment deposition during the operating life times using an FEM model. In addition the predicted temperatures are used to derive appropriate creep properties at relevant temperatures in a 3D pipe FEM creep analysis to predict the pipe deformation rate. All compare well with the actual service exposed pipe measurements and layer deposition. The overheated side revealed a small loss of creep strength in a stress rupture test. A layer of sediment (appr. 10 mm thickness) consisting basically of sintered carbon (coke) spread over the inside of the tube was acting as a thermal barrier causing the temperature to rise above 650 Cº. Analysis for the overheated side predicted an upper bound temperature of 800 Cº and a life of about 50 h suggesting that failure by creep rupture could occur rapidly in the sediment region.
International Journal of Engineering Research and Applications (IJERA) is an open access online peer reviewed international journal that publishes research and review articles in the fields of Computer Science, Neural Networks, Electrical Engineering, Software Engineering, Information Technology, Mechanical Engineering, Chemical Engineering, Plastic Engineering, Food Technology, Textile Engineering, Nano Technology & science, Power Electronics, Electronics & Communication Engineering, Computational mathematics, Image processing, Civil Engineering, Structural Engineering, Environmental Engineering, VLSI Testing & Low Power VLSI Design etc.
Effect of Quenching Media on Mechanical Properties for Medium Carbon SteelIJERA Editor
In this research work the mechanical properties of medium carbon steel has been studied . the Steel AISI 1039
quenched in different quenching media. These quenching media were cold water, water , oil and hot water.
Hardness , tensile , impact and wear tests have been carried out for specimens after quenching in different
media.
It was found that the tensile strength and hardness increased with increasing the heating temperature values of
heat treatment process. Also quenching in cold water has a great effect on tensile strength and hardness values .
where the heights value for tensile strength was (998.6N/mm²) and the hardness was (360.4 Hv) for steel which
quenching in cold water. The percentage of elongation decreased with increasing the temperature of heat
treatment process. also the lowest values of elongation was after quenching process in cold water.
However, the impact toughness and wear rate values were high for alloy after stress relief and lower after
quenching in different media. But the lowest values were recorded after quenching in cold water. It was found
that the absorbed energy and the wear rate for the alloy quenched in cold water were (23.6) J and
(2x10¯⁷gm/cm) respectively. While, for steels treated with the stress relief process were (62.02) J and
(7x10¯⁷gm/cm) respectively.
The effect of welding heat input and welding speed on microstructure of chrom...eSAT Publishing House
IJRET : International Journal of Research in Engineering and Technology is an international peer reviewed, online journal published by eSAT Publishing House for the enhancement of research in various disciplines of Engineering and Technology. The aim and scope of the journal is to provide an academic medium and an important reference for the advancement and dissemination of research results that support high-level learning, teaching and research in the fields of Engineering and Technology. We bring together Scientists, Academician, Field Engineers, Scholars and Students of related fields of Engineering and Technology
Effect of chromium powder mixed dielectric on performance characteristic of a...eSAT Journals
Abstract
In this paper, the effect of chromium powder mixed dielectric fluid on machining characteristics of AISI D2 die steel has been studied. Peak current, pulse on time, pulse off time, concentration of powder are the process parameters. The process performance is measured in terms of material removal rate (MRR), tool wear rate (TWR) and surface roughness (SR). The research outcome will identify the important process parameters that maximize MRR, minimize TWR and SR. The design of experiment has been undertaken using Taguchi method. ANOVA analysis has been used to investigate the percentage contribution of each process parameter for optimizing the performance. The study indicates that all the selected parameters except pulse off time have a significant effect on MRR. Current is found to be the most significant factor for MRR and TWR. With increase in current, TWR increases. Also, surface roughness increases with increase in pulse off time.
Keywords: PMEDM, Material removal rate, Tool wear rate, Surface roughness, Taguchi method
Effect of configuration on lateral displacement and cost of the structure for...eSAT Journals
Abstract
The choice of a cost effective lateral-force-resisting system for high-rise structures is challenging. There is no streamlined methodology to quantitatively compare the cost-effectiveness of each system beyond the more qualitative perception based evaluation of advantages or disadvantages. Developers currently base their decisions on architectural layout and structural integrity. Cost considerations are often primarily based on experience.
This decision making process has three primary shortfalls.
1) It may not incorporate factors which greatly affect the economy of a particular framing system.
2) It may not allow engineers to carryout designs at the least cost.
3) Comparison of framing systems may not address the specific building types.
This investigation proposes a prototype cost-effective model for selecting either a skeleton framing system or skeleton frame with bracing system for steel structural frames. A model for selecting cost-effective skeleton framing system or skeleton frame with bracing system will be a valuable tool for all decision makers. Engineers, in particular, will be able to select optimal steel framing faster, thus reducing design time and iterations. Furthermore, selection of economic framing system will also result in direct cost savings for steel structural frames.
The study involves the design and cost estimation of steel frames representing skeleton framing system and skeleton frame with bracingsystem. The cost effectiveness of the framing systems are compared based on lateral displacement requirements and cost.The preferred framing system should meet lateral displacement requirements and is lower in cost. The results of this pilot study showed that the Skelton framing system with bracing is the cost-effective choice for 30storeys steel space frames at wind speeds of 55m/sec, 50m/sec and 47m/sec.
Keywords: Bracings, SFS (Skeleton framing system), SFWB (Skeleton frame with bracing system) etc…
Effect of Heat Treatment on Corrosion Behavior of Spring SteelsEditor IJCATR
The experimental work deals with the effect of heat treatment on the corrosion behaviour of spring steels. In this study the
heat treatments like hardening, normalizing and tempering were done for spring steels to obtain martensitic matrix, pearlitic structure
and tempered martensitic matrix respectively. After heat treatment the microstructural studies were carried out for the samples using
SEM. Hardness measurements were done. The corrosion behaviour of all heat treated samples in HCl at different concentration (1.5N,
2N and 2.5N) was determined using Tafel extrapolation technique. The variation in the corrosion rates due to the effect of heat
treatment was noted. The results indicate that for fully martensitic matrix the corrosion rate is minimum and for pearlitic structure its
maximum. As tempering time is increased the corrosion rate increases correspondingly. The corroded microstructural images were
also taken using SEM and analysed.
Experimental and Finite Element Analysis of Single-V Groove Butt Weld on Weld...IJSRD
Gas Tungsten Arc Welding Process (GTAW) is widely used in fabrication of Aluminium and Aluminium Alloy material when precision is considered as a prime importance. Deformations in the object undergoing welding are one of the foremost problems encountered in the welding industry. Thus it is often required to study the factors which affect the deformations produced during welding to avoid errors in the geometry. Present investigation highlights Experimental and Finite Element Analysis of a Single-V Groove Butt Weld on Weld Pool Geometry of Aluminium Alloy Plate under Different Joint Parameters.Finite Element Method (FEM) has been employed to do the transient thermal and structural analysis of the assembly. The Finite Element Analysis has been done on ANSYS 14.5 Workbench. Number of factors is liable to produce effects in the job during the welding operation. Aim of this paper is the effect of welding parameters like as welding current, shielding gas flow rate and welding speed with mechanical Properties like tensile strength and hardness. After that finite element analysis for temperature distribution and distribution of the stresses in the welded Aluminium alloy plate. The results show that the larger the Welding current and smaller welding speed will lead to the maximum residual tensile stress. Therefore a residual stress will arise from the restraint position. The ultimate residual stress of weldment is determined by material yield strength at different temperature. The higher yield strength at different temperature has higher material residual stress. Because of its higher thermal conductivity, aluminium alloy test specimens have small temperature differential.
Studying the Fatigue Properties Of Hardened For Carbon Steelijceronline
In this study, Medium carbon steel is one of the most important materials used in industrial applications especially it is used in applications exposed to fatigue stresses such as airplanes, automotive components and electrical engines industries. Medium carbon steels were prepared and the effect of hardening on hardening strength of medium carbon steel was studied, the flame hardening method was used at different speeds then fatigue test was done. The following results were obtained, first sample (none), second sample (3.5 mm/s), and third sample (1.75 mm /s) and forth sample (1.165 mm/s). It has been found that as the flaming speed increases, the fatigue strength of the material decreases. The fatigue test result at stress (407.44 N/mm2 ) was as follow: for the first sample the no. of cycles to failure was at (67511 rpm), for the second sample (95832 rpm), for the third sample (122565rpm) and for the fourth sample it was (134585 rpm).
Parametric study of surface roughness in turning of az31 b mg alloy under dif...Imran Sarker
A study comprising of different surface roughness parameters of AZ31B Mg alloy was done in this experiment successfully. The study was done by turning AZ31B Mg alloy under varied feed, depth and cooling condition i.e., dry, conventional flood, MQL. Different amount of surface roughness was measured by the service of a roughness tester. The collected data from the turning operation were used to analyze and get desirable results on behalf of low surface roughness. The analysis was done by means of Taguchi method and the following results were shown:
The experimentation shows that, the cutting speed has insignificant impact on the studied surface roughness parameters.
Feed rate has significant influence over the surface roughness parameters. It expressed itself as the most dominant control factor to determine a better surface roughness parameter.
Depth of cut has insignificant influence over the surface roughness parameter and it has less effect on the roughness parameters compared to feed rate.
In cutting condition, MQL emerged as the major cooling condition compared to other two conditions which are dry and flood condition.
The future study can be conducted on the investigation of tool wear and chip morphology in turning of Mg AZ31B alloy under dry, flood and MQL conditions.
Influence of Heat Treatment on Mechanical Properties of Aisi1040 SteelIOSR Journals
This investigation is concerned to evaluate the influence of heat treatment on mechanical behavior of AISI1040 steel; it is one of the grades of medium carbon steel of American standard containing 0.40% carbon in its composition. Specimen of quenched/hardened AISI1040 steel was tempered at temperature (650,450&250℃) for 60, 90&120 minutes to modify desired properties. The mechanical behavior, particularly, ultimate tensile strength, yield strength and elongation were investigated using universal testing machine; while the hardness measurement was done on Rockwell hardness testing machine of heat treated specimens. Result shows that the ultimate tensile strength and the yield strength decrease while the elongation increases with an increase in tempering temperature and tempering time of different tempered specimen. The hardness of quenched/hardened specimen decreases with an increase in tempering temperature and tempering time. Furthermore, increasing temperature and lowering time produces approximately same result as decreasing temperature and increasing time.
Effect of cryogenic treatment on tool steel (aisi ¬d2)eSAT Journals
Abstract
In present scenario modernization of machine tools is on prime consideration that is an optimization of desired properties in machine tool parts means alternation of properties for that previously we employed heat treatment of steel, thus we have some improved properties but does not achieved correct solution for the problem. In modern age a new technology is comes on the front line, recognize by Acronyms C.T.P. or Cryogenic treatment of steel which has been done in cooling Atmosphere below Atmospheric tem. About – 1960C or- 3100F. During this temp. Range conversion of Austenite to marten site takes place. Thus we have got increased some desirable properties like reduced wear & Tear. Increased Hardness Micro- structure improved, Stress relieving properties also improved. In this paper tool Steel AISI- D2 is used for cryogenic treatment & study is performed regarding Micro- structure and Hardness, after Cryogenic treatment comparison is also made with un-treated test specimen.
Keywords:-AISI- D2, Cryogenic Treatment, Phase Transformation, Hardness, Micro- Structure
FellowBuddy.com is an innovative platform that brings students together to share notes, exam papers, study guides, project reports and presentation for upcoming exams.
We connect Students who have an understanding of course material with Students who need help.
Benefits:-
# Students can catch up on notes they missed because of an absence.
# Underachievers can find peer developed notes that break down lecture and study material in a way that they can understand
# Students can earn better grades, save time and study effectively
Our Vision & Mission – Simplifying Students Life
Our Belief – “The great breakthrough in your life comes when you realize it, that you can learn anything you need to learn; to accomplish any goal that you have set for yourself. This means there are no limits on what you can be, have or do.”
Like Us - https://www.facebook.com/FellowBuddycom
Remaining life assessment of refinery furnace tubes using finite element methodBarhm Mohamad
Crude oil heater 9Cre-1Mo steel tubes from a refinery plant were studied, after 5 years of service at nominally 650 Cº and 3 bar, to predict their remnant lives. The investigation included dimensional, hardness and tensile measurements in addition to accelerated stress rupture tests between 650 Cº and 700 Cº and microstructural examination. Tube specimens were taken from two sections, the overheated side and the side which only saw the nominal operating temperature. The method employed involved the prediction of the increase in temperature with increasing sediment deposition during the operating life times using an FEM model. In addition the predicted temperatures are used to derive appropriate creep properties at relevant temperatures in a 3D pipe FEM creep analysis to predict the pipe deformation rate. All compare well with the actual service exposed pipe measurements and layer deposition. The overheated side revealed a small loss of creep strength in a stress rupture test. A layer of sediment (appr. 10 mm thickness) consisting basically of sintered carbon (coke) spread over the inside of the tube was acting as a thermal barrier causing the temperature to rise above 650 Cº. Analysis for the overheated side predicted an upper bound temperature of 800 Cº and a life of about 50 h suggesting that failure by creep rupture could occur rapidly in the sediment region.
International Journal of Engineering Research and Applications (IJERA) is an open access online peer reviewed international journal that publishes research and review articles in the fields of Computer Science, Neural Networks, Electrical Engineering, Software Engineering, Information Technology, Mechanical Engineering, Chemical Engineering, Plastic Engineering, Food Technology, Textile Engineering, Nano Technology & science, Power Electronics, Electronics & Communication Engineering, Computational mathematics, Image processing, Civil Engineering, Structural Engineering, Environmental Engineering, VLSI Testing & Low Power VLSI Design etc.
Effect of Quenching Media on Mechanical Properties for Medium Carbon SteelIJERA Editor
In this research work the mechanical properties of medium carbon steel has been studied . the Steel AISI 1039
quenched in different quenching media. These quenching media were cold water, water , oil and hot water.
Hardness , tensile , impact and wear tests have been carried out for specimens after quenching in different
media.
It was found that the tensile strength and hardness increased with increasing the heating temperature values of
heat treatment process. Also quenching in cold water has a great effect on tensile strength and hardness values .
where the heights value for tensile strength was (998.6N/mm²) and the hardness was (360.4 Hv) for steel which
quenching in cold water. The percentage of elongation decreased with increasing the temperature of heat
treatment process. also the lowest values of elongation was after quenching process in cold water.
However, the impact toughness and wear rate values were high for alloy after stress relief and lower after
quenching in different media. But the lowest values were recorded after quenching in cold water. It was found
that the absorbed energy and the wear rate for the alloy quenched in cold water were (23.6) J and
(2x10¯⁷gm/cm) respectively. While, for steels treated with the stress relief process were (62.02) J and
(7x10¯⁷gm/cm) respectively.
The effect of welding heat input and welding speed on microstructure of chrom...eSAT Publishing House
IJRET : International Journal of Research in Engineering and Technology is an international peer reviewed, online journal published by eSAT Publishing House for the enhancement of research in various disciplines of Engineering and Technology. The aim and scope of the journal is to provide an academic medium and an important reference for the advancement and dissemination of research results that support high-level learning, teaching and research in the fields of Engineering and Technology. We bring together Scientists, Academician, Field Engineers, Scholars and Students of related fields of Engineering and Technology
Effect of chromium powder mixed dielectric on performance characteristic of a...eSAT Journals
Abstract
In this paper, the effect of chromium powder mixed dielectric fluid on machining characteristics of AISI D2 die steel has been studied. Peak current, pulse on time, pulse off time, concentration of powder are the process parameters. The process performance is measured in terms of material removal rate (MRR), tool wear rate (TWR) and surface roughness (SR). The research outcome will identify the important process parameters that maximize MRR, minimize TWR and SR. The design of experiment has been undertaken using Taguchi method. ANOVA analysis has been used to investigate the percentage contribution of each process parameter for optimizing the performance. The study indicates that all the selected parameters except pulse off time have a significant effect on MRR. Current is found to be the most significant factor for MRR and TWR. With increase in current, TWR increases. Also, surface roughness increases with increase in pulse off time.
Keywords: PMEDM, Material removal rate, Tool wear rate, Surface roughness, Taguchi method
Effect of configuration on lateral displacement and cost of the structure for...eSAT Journals
Abstract
The choice of a cost effective lateral-force-resisting system for high-rise structures is challenging. There is no streamlined methodology to quantitatively compare the cost-effectiveness of each system beyond the more qualitative perception based evaluation of advantages or disadvantages. Developers currently base their decisions on architectural layout and structural integrity. Cost considerations are often primarily based on experience.
This decision making process has three primary shortfalls.
1) It may not incorporate factors which greatly affect the economy of a particular framing system.
2) It may not allow engineers to carryout designs at the least cost.
3) Comparison of framing systems may not address the specific building types.
This investigation proposes a prototype cost-effective model for selecting either a skeleton framing system or skeleton frame with bracing system for steel structural frames. A model for selecting cost-effective skeleton framing system or skeleton frame with bracing system will be a valuable tool for all decision makers. Engineers, in particular, will be able to select optimal steel framing faster, thus reducing design time and iterations. Furthermore, selection of economic framing system will also result in direct cost savings for steel structural frames.
The study involves the design and cost estimation of steel frames representing skeleton framing system and skeleton frame with bracingsystem. The cost effectiveness of the framing systems are compared based on lateral displacement requirements and cost.The preferred framing system should meet lateral displacement requirements and is lower in cost. The results of this pilot study showed that the Skelton framing system with bracing is the cost-effective choice for 30storeys steel space frames at wind speeds of 55m/sec, 50m/sec and 47m/sec.
Keywords: Bracings, SFS (Skeleton framing system), SFWB (Skeleton frame with bracing system) etc…
Effect of Heat Treatment on Corrosion Behavior of Spring SteelsEditor IJCATR
The experimental work deals with the effect of heat treatment on the corrosion behaviour of spring steels. In this study the
heat treatments like hardening, normalizing and tempering were done for spring steels to obtain martensitic matrix, pearlitic structure
and tempered martensitic matrix respectively. After heat treatment the microstructural studies were carried out for the samples using
SEM. Hardness measurements were done. The corrosion behaviour of all heat treated samples in HCl at different concentration (1.5N,
2N and 2.5N) was determined using Tafel extrapolation technique. The variation in the corrosion rates due to the effect of heat
treatment was noted. The results indicate that for fully martensitic matrix the corrosion rate is minimum and for pearlitic structure its
maximum. As tempering time is increased the corrosion rate increases correspondingly. The corroded microstructural images were
also taken using SEM and analysed.
Experimental and Finite Element Analysis of Single-V Groove Butt Weld on Weld...IJSRD
Gas Tungsten Arc Welding Process (GTAW) is widely used in fabrication of Aluminium and Aluminium Alloy material when precision is considered as a prime importance. Deformations in the object undergoing welding are one of the foremost problems encountered in the welding industry. Thus it is often required to study the factors which affect the deformations produced during welding to avoid errors in the geometry. Present investigation highlights Experimental and Finite Element Analysis of a Single-V Groove Butt Weld on Weld Pool Geometry of Aluminium Alloy Plate under Different Joint Parameters.Finite Element Method (FEM) has been employed to do the transient thermal and structural analysis of the assembly. The Finite Element Analysis has been done on ANSYS 14.5 Workbench. Number of factors is liable to produce effects in the job during the welding operation. Aim of this paper is the effect of welding parameters like as welding current, shielding gas flow rate and welding speed with mechanical Properties like tensile strength and hardness. After that finite element analysis for temperature distribution and distribution of the stresses in the welded Aluminium alloy plate. The results show that the larger the Welding current and smaller welding speed will lead to the maximum residual tensile stress. Therefore a residual stress will arise from the restraint position. The ultimate residual stress of weldment is determined by material yield strength at different temperature. The higher yield strength at different temperature has higher material residual stress. Because of its higher thermal conductivity, aluminium alloy test specimens have small temperature differential.
Studying the Fatigue Properties Of Hardened For Carbon Steelijceronline
In this study, Medium carbon steel is one of the most important materials used in industrial applications especially it is used in applications exposed to fatigue stresses such as airplanes, automotive components and electrical engines industries. Medium carbon steels were prepared and the effect of hardening on hardening strength of medium carbon steel was studied, the flame hardening method was used at different speeds then fatigue test was done. The following results were obtained, first sample (none), second sample (3.5 mm/s), and third sample (1.75 mm /s) and forth sample (1.165 mm/s). It has been found that as the flaming speed increases, the fatigue strength of the material decreases. The fatigue test result at stress (407.44 N/mm2 ) was as follow: for the first sample the no. of cycles to failure was at (67511 rpm), for the second sample (95832 rpm), for the third sample (122565rpm) and for the fourth sample it was (134585 rpm).
Parametric study of surface roughness in turning of az31 b mg alloy under dif...Imran Sarker
A study comprising of different surface roughness parameters of AZ31B Mg alloy was done in this experiment successfully. The study was done by turning AZ31B Mg alloy under varied feed, depth and cooling condition i.e., dry, conventional flood, MQL. Different amount of surface roughness was measured by the service of a roughness tester. The collected data from the turning operation were used to analyze and get desirable results on behalf of low surface roughness. The analysis was done by means of Taguchi method and the following results were shown:
The experimentation shows that, the cutting speed has insignificant impact on the studied surface roughness parameters.
Feed rate has significant influence over the surface roughness parameters. It expressed itself as the most dominant control factor to determine a better surface roughness parameter.
Depth of cut has insignificant influence over the surface roughness parameter and it has less effect on the roughness parameters compared to feed rate.
In cutting condition, MQL emerged as the major cooling condition compared to other two conditions which are dry and flood condition.
The future study can be conducted on the investigation of tool wear and chip morphology in turning of Mg AZ31B alloy under dry, flood and MQL conditions.
Influence of Heat Treatment on Mechanical Properties of Aisi1040 SteelIOSR Journals
This investigation is concerned to evaluate the influence of heat treatment on mechanical behavior of AISI1040 steel; it is one of the grades of medium carbon steel of American standard containing 0.40% carbon in its composition. Specimen of quenched/hardened AISI1040 steel was tempered at temperature (650,450&250℃) for 60, 90&120 minutes to modify desired properties. The mechanical behavior, particularly, ultimate tensile strength, yield strength and elongation were investigated using universal testing machine; while the hardness measurement was done on Rockwell hardness testing machine of heat treated specimens. Result shows that the ultimate tensile strength and the yield strength decrease while the elongation increases with an increase in tempering temperature and tempering time of different tempered specimen. The hardness of quenched/hardened specimen decreases with an increase in tempering temperature and tempering time. Furthermore, increasing temperature and lowering time produces approximately same result as decreasing temperature and increasing time.
Effect of cryogenic treatment on tool steel (aisi ¬d2)eSAT Journals
Abstract
In present scenario modernization of machine tools is on prime consideration that is an optimization of desired properties in machine tool parts means alternation of properties for that previously we employed heat treatment of steel, thus we have some improved properties but does not achieved correct solution for the problem. In modern age a new technology is comes on the front line, recognize by Acronyms C.T.P. or Cryogenic treatment of steel which has been done in cooling Atmosphere below Atmospheric tem. About – 1960C or- 3100F. During this temp. Range conversion of Austenite to marten site takes place. Thus we have got increased some desirable properties like reduced wear & Tear. Increased Hardness Micro- structure improved, Stress relieving properties also improved. In this paper tool Steel AISI- D2 is used for cryogenic treatment & study is performed regarding Micro- structure and Hardness, after Cryogenic treatment comparison is also made with un-treated test specimen.
Keywords:-AISI- D2, Cryogenic Treatment, Phase Transformation, Hardness, Micro- Structure
FellowBuddy.com is an innovative platform that brings students together to share notes, exam papers, study guides, project reports and presentation for upcoming exams.
We connect Students who have an understanding of course material with Students who need help.
Benefits:-
# Students can catch up on notes they missed because of an absence.
# Underachievers can find peer developed notes that break down lecture and study material in a way that they can understand
# Students can earn better grades, save time and study effectively
Our Vision & Mission – Simplifying Students Life
Our Belief – “The great breakthrough in your life comes when you realize it, that you can learn anything you need to learn; to accomplish any goal that you have set for yourself. This means there are no limits on what you can be, have or do.”
Like Us - https://www.facebook.com/FellowBuddycom
Comparison of Mechanical Properties of Austempered, Normalized and As-Weld Ca...IJAEMSJORNAL
More often than not, welded joints experience failure such as fracture which jeopardize their reliability and ergonomics when put in perspective. Attempting a significant improvement in the mechanical properties of welded joint through heat treatment could ensure joints stability and reduce the costs associated with constant repairs and replacements. In this study, the effects of heat treatments (austempering and normalization) on the mechanical properties of weldments were examined. The locally recycled steel sample was sourced from the Delta Steel Company Aladja, Delta State and the spectro-analysis was carried out on it. The test samples were machined as per properties for tests, fractured locally and were welded using shielded metal arc welding (SMAW) with stainless steel electrode. They were then heat treated in electric furnaces. The mechanical properties (tensile strength, yield strength, hardness and impact toughness) were determined and the microstructure examined using scanning electron microscope. They were also examined physically using hand lens. The result indicated that the austempered samples improved significantly in terms of its tensile strength, yield strength, hardness and ductility. It was also found that the untreated sample produced the greatest impact toughness. The result of the physical examination also suggested that heat treatment using oil based quenchant have the potential to inhibit rust at weld joints.
Effects of Continuous Cooling On Impact and Micro Structural Properties of Lo...IJMER
Some mechanical properties and microstructural analysis were conducted on shielded
metal arc weldments of low carbon steels in some simulated environments. Specimens were prepared
and subjected to welding and continuous cooling at the same time at various positions. Results obtained
for impact strength using Charpy impact testing machine showed that impact strength of water cooled
samples were higher compared to salty water cooled samples. This is due to the increased formation of
martensitic structure and finer pearlite grains. The microstructure of the samples was studied using
photographic visual metallurgical microscope. For low cooling rate as in the air cooled sample, the
austenite was observed to transform into ferrite and pearlite. Ferrite is a body-centred cubic crystal
structure of iron alloys. For higher cooling rates of water and salt water cooled samples, low
temperature transformation products like bainite (an acicular microstructure which is not a phase) or
martensite (a very hard form of steel crystalline structure) were formed. The salt water cooled samples
had more martensite regions because of the increased cooling rate
Some Results from the Investigation of Effects of Heat Treatment on Propertie...IJERDJOURNAL
Abstract:- The results of an investigation which was undertaken to reveal the differences in the mechanical properties and microstructural characteristics of two types of Ni-hard cast irons are presented in this study. The cast irons were obtained in a laboratory conditions and their compositions are in accordance with European standard EN 12513. One type of cast iron is EN GJN-HV520 (Ni-hard 2) containing 2.10% Cr and the second type EN GJN-HV600 (Ni-hard 4) with 9.04% Cr. The cast irons were evaluated in both as-cast and heat treated conditions. To improve mechanical properties specifically wear resistance, the samples of both types Ni-hard cast irons were subjected to different heat treatment processes. Annealing of Ni-hard 2 samples at 480°C during 4 hours caused increasing of hardness for about 13.5% due to additional precipitation of secondary carbides. On the other hand the heat treatment process consisting of annealing at 790°C during 4-8 hours of Ni-hard 4 samples, compared to the as-cast condition, improve the hardness for about 22.5%. In this case besides precipitation of secondary carbides, transformation of retained austenite to martensite occurs.
DEVELOPMENT OF DUAL PHASE STEEL AND DETERMINATION OF IT'S MECHANICAL PROPERTI...IAEME Publication
In this paper, the development of dual phase steel from low carbon steel and mechanical properties have been studies. Dual phase steel is developed by intercritical annealing in order to improve the hardness and impact toughness. Low carbon steel of 0.21% carbon content is first intercritically heated in furnace and then rapid cooling in water is done to obtain the martensitic steels. Different samples of DP steels are prepared by the intercritical annealing process temperature ranging from740˚C to 840˚C. The heating temperature and different time of heating of the steel is
used to make different percentage of Maternsite steel.
Finite Element Simulation of Plasma Transferred ARC Welding [PTAW] of Structu...IJERA Editor
Plasma transferred Arc welding is one of the most widely used welding process, in which the metals are fused just above the melting point, and makes the metal to fuse. It is employed in many applications like tool die and metal casting, strip metal welding etc. This investigation is to analyze temperature distribution residual stress and distortion by varying the heat source parameter in SYSWELD, and compared the results with ANSYS. The simulation of Plasma Transferred Arc welding was of structural steel plate performed using a non-linear transient heat transfer analysis. Heat losses due to convection and variation of material properties with temperature were considered in this analysis. To incorporate the heat developed the Gaussian distribution was considered. Finite element simulations were performed using ANSYS Parametric Design Language (APDL) code and using SYSWELD. The temperatures obtained were compared with experimental results for validation. It was found that the predicted values of temperature agree very well with the experimental values. Residual Stress and Distortion were also predicted for various heat Input. The effect of heat input on residual stress and distortion was investigated.
International Journal of Engineering Research and Applications (IJERA) is an open access online peer reviewed international journal that publishes research and review articles in the fields of Computer Science, Neural Networks, Electrical Engineering, Software Engineering, Information Technology, Mechanical Engineering, Chemical Engineering, Plastic Engineering, Food Technology, Textile Engineering, Nano Technology & science, Power Electronics, Electronics & Communication Engineering, Computational mathematics, Image processing, Civil Engineering, Structural Engineering, Environmental Engineering, VLSI Testing & Low Power VLSI Design etc.
MECHANICAL PROPERTY ASSESSMENT OF AUSTEMPERED AND CONVENTIONALLY HARDENED AIS...IAEME Publication
The chemical composition and mechanical properties of steel decide its applicability for manufacturing various components in different areas of engineering interests. Heat treatment processes are commonly used to enhance the required properties of steel with or without change in chemical composition. The present work aims to perform conventional hardening and Austempering treatment with experimental investigation of the effect of austempering and conventional hardening (quenching) on AISI 4340 steel. Different tests like tensile, torsion, hardness, impact and microstructure analysis are carried out in as bought and heat treated conditions
Effect of Hardness and Wear Resistance on En 353 Steel by Heat Treatment IJMER
En 353 steel is an easily available and cheap material that is acceptable for heavy duty
applications. Heat treatment on En 353 steel is improved the ductility, toughness, strength, hardness and
relive internal stress in the material. Spectrographic method is used to analyze the composition of the
alloy material. The experimental results of hardness and dry wear testing on pin-on-disc are done to get
idea about heat treated En 353 steel. It is found that the hardness and wear resistance of the En 353 steel
is improved after the heat treatment and the microstructure is changed from ferrite to martensite.
A Comparative Study on Direct and Pulsed Current Gas Tungsten Arc Welding of ...IDES Editor
the aim of this article is to evaluate the mechanical
and microstructure properties of Inconel 617 weldments
produced by direct current electrode negative (DCEN) gas
tungsten arc welding (GTAW) and pulse current GTAW. In
this regard, the micro structural examinations, impact test
and hardness test were performed. The results indicated that
the joints produced by direct mode GTAW exhibit poor
mechanical properties due to presence of coarse grains and
dendrites. Grain refining in pulse current GTAW is reason of
higher toughness and impact energy than DCEN GTAW.
Further investigations showed that the epitaxial growth is
existed in both modes that can strongly affect the mechanical
behavior of the joints in heat affected zone (HAZ).
Role of Coating in Improving High Temperature Oxidation of SteelIJERD Editor
Oxidation is the major degradation mechanism of failure for various components operating at high
temperature. Protective coatings are used to improve the oxidation resistance of such component. In the present
investigation, Al2O3 and Ni-20Cr coatings have been deposited on SAE431 boiler steel by Detonation Gun
Spraying Method. The oxidation performance of Al2O3 and Ni-20Cr coated as well as uncoated SAE-431 steel
has been evaluated in air under cyclic conditions at an elevated temperatures of 8000C. Al2O3 coating on
SAE431 boiler steel has shown approximately 26% improvement in the oxidation resistance of SAE431 steel
whereas Ni-20Cr coating on SAE431 boiler steel has indicated about 21% improvement in the oxidation
resistance as compared to the uncoated SAE431 boiler steel.
Similar to A Differential Scanning Calorimetry (DSC) study of welding consumables for modified 9Cr-1Mo ferritic steel (20)
Role of Coating in Improving High Temperature Oxidation of Steel
A Differential Scanning Calorimetry (DSC) study of welding consumables for modified 9Cr-1Mo ferritic steel
1. 1
IIWIC 2008, Chennai 8-10, Jan. 2008 370-380
A Differential Scanning Calorimetry (DSC) study of welding
consumables for modified 9Cr-1Mo ferritic steel
B. Jeyaganesh1
, S. Raju1*
, S. Murugesan, E. Mohandas1
,
M. Vijayalakshmi1
, V. Ramasubbu2
, S. K. Albert2
and A. K. Bhaduri2
1
Physical Metallurgy Division,
2
Materials Technology Division
Indira Gandhi Centre for Atomic Research (IGCAR), Kalpakkam, 603 102, India
• Corresponding Author; E-mail : sraju@igcar.gov.in
• Tel : 91 44 27480306; Fax : 91 44 274 80 081
Abstract
A comprehensive characterisation of the thermal stability of four welding
consumables that are developed for welding mod. 9Cr-1Mo steel has been performed
using DSC. The various transformation arrest points such as Ac1, Ac3, the solidus and
liquidus temperatures and the enthalpy effects associated with the α→γ phase change
and melting have been determined precisely. It is found that both Ac1 and Ac3
temperatures exhibit a decrease with increasing (Mn+Ni) content. In addition, the
kinetics of austenite formation from a tempered martensitic microstructure has been
modelled in terms a simple isochronal version of the Kolmogorov-Johnson-Mehl-
Avrami (KJMA) formalism for the nucleation and growth phenomenon. It is found
that the apparent activation energy for austenite formation is sensitive to the heating
rate, in that the activation energy is more for slower rates of heating. An apparent
activation energy of about 260 kJ mol-1
is suggested for the α→γ transformation in
high chromium steels
(Key words : mod. 9Cr1Mo steel, welding electrode, phase transformation, DSC, activation energy)
2. 2
1.0. Introduction
A study on ferritic steels is of interest on both and applied grounds. On the
application front front, the use of Cr –Mo based ferritic steels in fossil fuel power
plants has a long history [1]. The combination of good thermal conductivity and low
thermal expansion [2] of ferritic alloys is particularly attractive from the point of view
of minimising the hazard from thermal stresses [1,3]. Besides, ferritic steels also
possess fairly good oxidation resistance at intermediate temperatures [3]. More over
the relatively low cost of ferritics as compared to 300- series of high nickel austenitic
stainless steels is an added economic incentive. The emerging pressure from both
economical and ecological quarters to enhance the thermal efficiency of conventional
fossil fuel fired power plants has only re-emphasised the need for developing
advanced grades of ferritic alloys that can function for longer durations at higher
temperatures, in the range 600 - 650 0
C [1,4]. The improved neutron irradiation
swelling resistance of ferritics over austenitic steels has also made them the preferred
choice as core structural candidates for realising an extended fuel burn up in liquid
metal cooled fast reactors, employing metallic fuels [5]. As a passing remark, we may
also note that ferritic steels have aroused significant interest among the fusion reactor
materials community as potential plasma facing first wall material [6]. On the basic
front, the various phase transformations that occur in ferritic steels as a function of
both temperature and composition and their influence on resulting microstructure
constitute an interesting play field for studying many physical metallurgical
phenomena.
It is a well-known fact that welding constitutes a major step in the fabrication of
power plant components. Therefore designing suitable welding process and welding
consumables in conjunction with appropriate pre and post weld heat treatment
3. 3
(PWHT) procedures is essential in ensuring quality welds. The advent of the newer
grades of ferritic steels in nuclear materials scenario [6-11] has catalysed an extensive
basic research programme on welding metallurgy, especially on those aspects that are
related to tailoring of composition of welding consumables with a view to minimise,
or avoid if possible, the formation of delta ferrite during the course of primary weld
solidification [12, 13]. Thus for example, a primary austenitic solidification mode
may be ensured by adjusting the combined concentration of austenite stabilising
elements such as, (Ni + Mn + Co + Cu + N + . .) in the overall composition of
welding consumables [13]. In some cases, the partial replacement of Mo by W, a
comparatively weak ferrite stabiliser [14], is also practised in addition so that
preferably nil or only a small delta ferrite is retained at the end welding process [15].
It must also be kept in mind that in tailoring the compositional limit of austenite
stabilisers, the attending penalty on the resulting low Ac1 transformation temperature
must also be given due consideration, for Ac1 decides the theoretical upper limit for
the post weld heat treatment (PWHT) temperature [13, 16, 17]. In addition to what has
been argued above, an appropriate balancing of the composition of welding
consumable is also called for in ensuring proper tempering of martensite during
PWHT, since the tempered microstructure resulting from the adoption of a tempering
temperature that is marginally higher than Ac1 often leads to reduced fracture
toughness and embrittlement during service [17, 18]. Thus, argued in any manner, a
comprehensive metallurgical characterisation of welding consumables is called for
from the standpoint of drawing appropriate welding specification.
In the construction of India’s first 500 MWe prototype fast breeder reactor
(PFBR), mod. 9Cr-1Mo steel has been identified as the candidate for the steam
generator tubes. Towards the cause of devising appropriate welding procedure, a few
4. 4
welding consumables with carefully tailored compositions have been chosen and
tested. As part of the broad based characterisation programme, we have undertaken in
this study a detailed differential scanning calorimetry (DSC) investigation of the
thermal stability and phase transformation characteristics of the welding consumables.
The results of this study are reported in this paper.
2.0. Experimental Procedure
2.1. Chemical composition, weld pad preparation and metallography
In table 1, the chemical composition of the four welding consumables, as
determined by direct reading optical emission spectroscopy is listed. These
consumables are : the E 9016 shielded metal arc welding (SMAW) electrodes
obtained from Kobe, Boehler and Midhani (E9016 – B9) and the filler wire for gas
tungsten arc welding (GTAW) obtained from M/S. Midhani, India. For comparison,
the composition of the base metal has also been presented in table 1.
A weld pad of dimension, 100 × 75 × 12 mm is made by the SMAW process for
the electrodes and by the GTAW method for the filler wire using the stringer bead
technique. A total of eight layers were built without any interpass treatment. The
following process parameters are adopted in making the weld pads: 90 A/25 V, heat
input of 900 – 1000 J for SMAW of electrodes; and 80 A/15 V, heat input of 300 J for
GTAW of the Midhani filler wire [19].
The samples for the present study were sliced from the portion that is located
approximately 2 mm below the top surface of the weld pad. For optical metallographic
characterisation, the specimens were prepared in the standard manner, starting from
coarse dry grinding to 1000 grade emery polishing and then to final finishing with
alumina and diamond polish. These were given a mild initial etching with a 2% nital
solution and then subsequently by the Villela’s reagent for about a minute. These
5. 5
polished samples were also used for x-ray diffraction (INEL, Cu Kα,) studies and
microhardness (Leitz, 100 g) measurements (table 2).
2.2. DSC experiments
The samples for DSC experiments were cut from the thin sections sliced originally
from the weld pad using diamond coated wire saw. These were further cleaned and
polished to regular and nearly identical cubes of mass varying from 50 to 70 ± 0.1 mg.
The DSC experiments were performed with Setaram Setsys 16®
heat-flux type high-
temperature differential scanning calorimeter, employing recrystallised alumina
crucibles of about 100µ L volume. The crucibles were ultrasonically cleaned in
methanol and rinsed with dilute HCl to remove any trace of contaminants arising from
previous use. The equipment details as well as the calibration procedure have been
discussed in our previous publication [20, 21]. Stated briefly, the experiments were
performed under a constant flow (50 ml per minute) of high purity argon. A range of
heating rates varying from 1 to of 100 K per minute is employed. While lower heating
rates (1-2 K min-1
) resulted in mild decarburisation of the sample due to the
appreciable resident time at high temperatures, high heating rates induce significant
thermal lag between the actual sample temperature and that sensed by the non-contact
probe. However, by calibrating the sample signal against the pure iron (Fe- Aldrich,
impurities ≤ 80 ppm) reference signal, especially around the region of phase
transitions, the temperature lag has been duly accounted for. It is generally found in
the case of 9Cr –1Mo ferritic steels, that for a heating rate of about 10 K min-1
, the
thermal lag is of the order of ≤ 2 K [22]. The sample mass and shape have been kept
nearly the same for both the reference and steel samples used in each set of
experiments. Fresh samples were used for each run, and multiple runs under identical
conditions are performed for calibrating the precision of the measured transformation
6. 6
temperature. The temperature calibration is performed using recommended high pure
melting point standards, namely, Sn, Al, Pb, In and Au. In addition, the measurement
of the enthalpy of α (bcc) → γ (fcc) allotropic transformation in pure iron under
identical experimental conditions is also employed for the heat flow calibration [22].
The heat flow rate or specific heat calibration is performed using the literature data on
the specific heat of pure iron [23, 24]. The measured transformation temperatures are
accurate to ± 1 K; and the transformation enthalpies even on a conservative estimate
are accurate to ± 5 % at 10 K min-1
. Since, a reliable and reproducible temperature and
heat flow calibration of DSC for cooling cycle is comparatively a difficult proposition
[25] due to the absence of reliable high temperature standards with known degrees of
undercooling, the enthalpy and the heat flow calibration of the signal were carried out
only for the heating cycle in the present study. It is presumed that the accuracy of
sample temperature measurement during cooling cycle is just the same as that of the
heating cycle [22].
3.0. Results
3.1. Optical microscopy, microhardness and x-ray diffraction studies
In figure 1(a-e), the optical micrographs of the three electrodes obtained from
Kobe, Boehler and Midhani and the filler wire supplied by Midhani are presented.
The characteristic martensite microstructure is generally seen in all the cases.
Although, no interpass treatment is allowed in the present study, the samples having
been sliced at about 2 mm below the top surface, might have suffered a mild auto
tempering due to the heat effects generated during subsequent welding passes. In the
case of Boehler electrode (fig 1a), the presence of a nicely outlined prior austenite
grain structure with some sporadic coarse carbide particles is readily apparent. The
microstructure of the Kobe electrode (fig 1b) on the other hand reveals a finer lath
7. 7
structure with no clear traces of prior austenite boundaries. The midhani electrode (fig
1c) reveals a coarser and somewhat patchy martensite while the microstructure of the
filler wire (fig. 1d) indicates considerable globularisation (fig. 1d). The base metal
microstructure (fig. 1e) is typical of tempered martensite with extensive decoration of
the ferrite subboundaries by numerous fine carbide particles. It should be mentioned
that this varying spectrum of microstructure witnessed at optical level is due to the
different extent of the residence time that each composition spends in different phase
fields during its thermal history [13]. In table 2 the microhardness values measured on
each sample under a load of 100 g are tabulated.
In figure 2, the room temperature x-ray diffraction profiles obtained using Cu-Kα
radiation for different samples are stacked together. The predominant peaks of α-
ferrite are clearly marked. Besides, a few very weak reflections from the (Fe,Cr)23C6
are also observed [26]. The estimated lattice parameter for the α-ferrite phase is found
to be 0. 2876 ± 0.0003 nm. It may be noted that this value is nearly the same for all
the welding consumables and is in agreement with that observed for 9Cr-1Mo low
carbon steel [20].
3.2. DSC studies : transformation temperatures and transformation enthalpy
In figure 3(a) a typical DSC profile obtained with the Midhani electrode is
illustrated. In 3(b), an exclusive, expanded view around the high temperature region is
illustrated for all the four welding consumables. In order to avoid clutter and needless
proliferation of figures, the thermogram of only one electrode composition is shown
in fig. 3(a). The details for others are tabulated (table 3). It must be mentioned that the
qualitative features of the DSC profiles are much the same for all compositions. Only
the onset and peak temperature values of various phase transformations are dependent
on the composition. A careful inspection of figure 3(a) reveals the following sequence
8. 8
of phase changes that take place upon slow heating (3 K min-1
) of a tempered
martensitic microstructure.
(i) ferromagnetic to paramagnetic transformation at TC, the curie point
of the α-ferrite phase. Depending on the composition, TC is found to
vary from 730 to 740 0
C. TC is more clearly attested during heating
than on cooling.
(ii) α-ferrite + M23C6 + MX → γ-austenite + M23C6 + MX
on crossing the Ac1 temperature. The transformation reaches a fair
degree of completion, depending on the heating rate, at Ac3. It has been
observed in high chromium steels that practically a little dissolution of
M23C6 alone is realised in this reaustenitisation step [27-30], although
the Thermo Calc®
based equilibrium simulations suggest small, yet
finite dissolution (5 %) by the time Ac3 is reached on very slow heating
[30-34].
(iii) γ + M23C6 + MX → γ + MX; (dissolution of M23C6 carbide).
Basically, the dissolution of carbide is a continuous reaction after
Ac3, and is generally seen as a shallow endothermic trough in an
otherwise smooth DSC profile [20]. This is observed better in slow
heating rate scans [22].
(iv) γ + MX → δ - ferrite + γ + MX; appearance of high temperature δ -
bcc phase.
(v) δ + γ + MX → δ + γ ; (dissolution of MX phase in γ )
(vi) δ + γ → liquid + δ + γ . (appearance of liquid)
(vii) liquid + δ + γ → liquid + δ (dissolution of γ in liquid)
(viii) liquid + δ → liquid (completion of melting)
9. 9
The region covered by the last three arrest points signifies the solidus – liquidus gap.
In the case of (9-12) Cr-Mo steels with a nominal carbon concentration of about 0.1
wt.%, the calculated equilibrium diagram(s) using Thermo Calc®
software and
associated steel database [34] suggests that one may encounter a very small existence
domain of the (liquid + δ + γ ) three phase field just prior to attaining the (δ + γ) two
phase region on slow continued heating [35]. The actual attainment is of course
dependent on kinetic factors [36]. This aspect has been kept in mind, while annotating
the high temperature region of the DSC profiles shown in figure 3(b). As can be seen,
the presence of a higher austenite stabilising (Mn + Ni + N) content in our weld
consumables as against the typical mod. 9Cr-1Mo base metal composition such as
P91 or E91, supports the possibility that a three phase (liquid + δ + γ ) equilibrium
field is in principle realised during slow (1-3 K min-1
) heating experiments. In figure
3(b), it is also interesting to note the subtle difference in the nature of the DSC
profiles for different consumables around (liquid + δ ) region. A somewhat flat
profile, such as the one witnessed for the midhani filler wire suggests that this
composition may be very close to the L + δ → L peritectic point, as compared to
other compositions. But this observation needs further scrutiny.
In the case of mod. 9Cr-1Mo steel, the M23C6 and MX phases refer
respectively to (Cr,Fe)23C6 and (V,Nb) (C,N) type mixed carbides and carbonitrides
[37, 38]. It must also be mentioned that for a given DSC instrument and a well
prescribed set of experimental conditions, the sharpness or the clearly defined nature
of various transformation arrest points is a direct function of the associated enthalpy
effect [25]. Unlike the case of α → γ structural transformation or melting, the other
phase changes such as the dissolution of M23C6 and MX phases, are accompanied by
only a meagre change in enthalpy [22]. Therefore, these changes manifest as mild yet
10. 10
distinct inflections in the base line compensated DSC profile [22]. In fact the various
transformation arrest temperatures are fixed by taking recourse to the derivative of the
actual DSC signal, in which these inflection points are more clearly marked.
The enthalpy effects associated with α → γ change and melting are given
directly in terms of the total area enclosed under the respective peak [39]. The
conversion factor required for getting enthalpy in terms of J g-1
is obtained from the
corresponding signal from pure iron [22]. The measured enthalpy values are listed in
the last two rows of table 3. As for the α → γ phase change is concerned, there is
reasonable agreement among the transformation enthalpy values recorded for the
midhani electrode, midhani filler wire and base metal. But the corresponding values
for both Kobe and Boehler electrodes are way of from this general trend. At this point,
it must be mentioned that for lower heating rates (1-10 K min-1
), the α → γ
transformation peak for the Kobe electrode is found to be very diffuse, contributing
thereby to a higher degree of uncertainty in the measured peak area and hence
enthalpy values. In addition, a critical inspection of the composition of Kobe electrode
suggests a relatively higher (Mn + Ni) content, which means the measured enthalpy
corresponds almost exclusively to the conversion of relatively destabilised ferrite into
austenite. In addition, the low carbon concentration of about 0.06 wt.% of Kobe
material supports the argument that it is exclusively the substitutionally alloyed ferrite
matrix that is getting transformed to austenite in the Ac1 – Ac3 intercritical domain;
any probable contribution from possible M23C6 dissolution is assumed to be nil in this
case. Both these factors can serve to decrease the enthalpy of α → γ phase change.
As for the melting enthalpy is concerned, the measured values are in the range 240 -
260 J g-1
. These values are of expected order and are in line with typical values
observed for low carbon alloy steels [40, 41].
11. 11
3.3. α-ferrite + carbides → γ-austenite transformation kinetics
Since α → γ phase change is a nucleation and growth controlled process, the
observed transformation onset and finish temperatures, namely Ac1 and Ac3 show
appreciable dependence on the rate of heating, β (Table 4). This point is graphically
illustrated in figure 4 for the midhani electrode. For other consumables, the relevant
data are listed in table 4. In figure 4(a), the change in the sharpness of the α → γ peak
profile with increasing heating rate is depicted. The methodology adopted for
obtaining Ac1 and Ac3 is also marked. In figure 4(b), the heating rate dependencies of
Ac1, Ac3 and Acα→γ peak temperatures are brought out. It is clear from this figure that
the transformation characteristics are strongly non linear in β, especially in the lower
range, of about 1-40 K min-1
. But this tendency reaches saturation for higher values of
β. With in the range of heating rates investigated in this study (100
to 102
K min-1
), the
variation of the transformation temperature with β can be satisfactorily expressed by
the following power law representation,
Tf (β) = To (β/βo)m
. (1)
In the above, Tf (β) stands for the general transformation temperature Tf measured as a
function of heating rate β, To is the transformation temperature for an arbitrarily
chosen reference heating rate (βo) and m is the power law exponent. For convenience,
βo may be taken as unity (βo = 1), and in which case, To becomes equal to the
observed transformation temperature at unit heating rate. From figure 4(b), it is
evident that Ac3 is more sensitive to the heating rate variation than Ac1, which
contributes to the kinetics induced widening of the (α + γ ) two phase field
(intercritical region) for higher heating rates. This is also inferred from the increasing
values of (Ac3-Ac1) with β (table 4). The reason for this behaviour is the fact that α
12. 12
→ γ transformation gets progressively difficult during its later stages, due possibly to
hard impingement effects which contributes to the delayed as well as incomplete
finishing of the transformation [42]. Although this is true for slow heating rates as
well, the steeply rising nature of Ac3 is however markedly evident for higher values of
β.
The fraction of austenite formed as a function of temperature γ(T) in the
intercritical zone (Ac1 ≤ T≤ Ac3) is estimated using the following expression
γ(T) = {Ac1∫T
ϕ dT) / (Ac1∫Ac3
ϕ dT)}. (2)
Here, Ac1∫T
ϕ dT, is the partial area under the peak in the temperature domain Ac1 – T.
The denominator Ac1∫Ac3
ϕ dT stands for the total peak area covering the entire
transformation temperature range. Eq. (2) assumes that austenite formation is
complete upon reaching Ac3, although this is not strictly true for higher heating rates
[42]. The transformation plots obtained using Eq. (2) are displayed in figure 5 for the
midhani electrode. It is clear that austenite formation from tempered martensite
supports the classical sigmoidal behaviour that is characteristic of a nucleation and
growth phenomenon.
In the usual methodology adopted for analysing the transformation kinetics on
continuous heating, the following functional form is often invoked to represent the
instantaneous reaction rate, (∂γ/∂T)β [43].
(∂γ/∂T)β = f(γ) k(T) (1/β). (3)
In this formalism, f(γ) is often taken to be an empirical, but suitable reaction model
that is consistent with the established kinetic features of the transformation under
consideration. The empirical rate constant k(T) is normally assumed to be the of the
Arrhenius form
k = k0 exp(-Qeff/RT), (4)
13. 13
with Qeff being the effective or apparent activation energy for the overall
transformation process. In a formal theoretical development of the overall
transformation kinetics for a nucleation and growth process, Qeff is actually identified
with a physically based model of nucleation and growth [44] and in such a case it can
be shown that it is actually a weighted sum of individual activation energies involved
in nucleation and growth processes [45-47]. For the case of α → γ transformation, the
activation energy for nucleating the γ phase, namely QN, is much smaller than that
involved in propagating the γ/α interface into ferrite QG [48-50]. In deference to the
overall scope of this study, the theoretical treatment of the transformation rate will not
be discussed here; nevertheless, it is sufficient to note that relative values of Qeff can
be given a consistent interpretation.
In the present study, the overall transformation kinetics is fitted to the following
nonisothermal version of the Kolmogorov-Johnson-Mehl-Avrami (KJMA) form for
the fraction of austenite γ(T) formed as a function of temperature at a constant heating
rate [46].
γ (T) = 1-exp{-kn
[R(T-TS)2
/β Qeff]n
}. (5)
It may be noted that in the above model, we have chosen T-TS, the temperature
increment with respect to the experimentally observed threshold or onset temperature
(TS) as the independent variable, since this corrects in an apparent manner for the
error incurred in not accounting precisely for the true start of the transformation
corresponding to zero transformed fraction. The experimental data on γ(T) for
different heating rates (β) are fitted using Eq. (5) by means of a standard nonlinear
optimisation routine and the resulting values for the kinetic quantities namely Qeff, k0,
and n are listed in table 5. As may be judged from this table, that notwithstanding the
14. 14
difference in composition, there is a nice agreement seen among the Qeff values
obtained for different consumables. The average value of n, the avrami exponent for
the overall transformation kinetics is about one. It also emerges from table 5, that the
kinetic parameters are somewhat sensitive to the heating rate; in particular the
apparent activation energy Q exhibits a gentle decrease with increasing heating rate
(β). While this point will be addressed in the discussion section, it is sufficient to note
that a standard KJMA model is able to account for the observed transformation
kinetics.
4.0. Discussion
4.1. Mn +Ni dependence of Ac1 temperature
One of the major outcomes of this investigation is the elucidation of the effect
of (Mn+Ni) content on the transformation temperatures. From the point of view of
welding physical metallurgy of high chromium ferritic-martensitic steels, two basic
considerations contribute to the proper choice of the welding consumable
composition. They are:
(i). the nature of the primary solidification mode, which needs to be austenitic
and
(ii). the on-heating Ae1 or Ac1 temperature, an appropriate value of which
decides the PWHT schedule. A standard manifestation of the balancing influence
between ferrite and austenite stabilising elements is the resulting Ac1 temperature.
Besides, the knowledge of Ac3 is also called for in rationalising the process related
heat treatments like homegenisation, normalising or any other hot working that is
done in the fully austenitic phase field. These metallurgical requirements are easily
satisfied by going in for a slightly higher quantum of austenite stabilising elements in
the overall composition. But an arbitrary enhancement of austenite stability by the
15. 15
way of increasing for example the combined (Mn+Ni) content is not recommended;
since this option interferes with the PWHT temperature and also results in
concomitant lowering of MS, the martensite start temperature and hence comes in the
way of realising a fully martensite structure in weld deposits [51]. The presence of a
duplex microstructure is inimical to toughness, creep ductility and so on [52].
The present study clearly reveals the role of combined (Mn+Ni) content in
lowering the Ac1 temperature in arc welding consumables as compared to the base
metal (figure 6). The present results on Ac1, can be satisfactorily fitted to the
following empirical relation
(Ac1/o
C) = 855 – 25.9 (Mn+Ni / wt.% ) – 4.0 (Mn+Ni/ wt.% )2
. (6)
Unfortunately, the number of data points catering to different (Mn+Ni) levels is too
small to support a statistical analysis; but nevertheless, the qualitative trend advocated
is in accord with the basic tenets of metallurgy. Further work on other compositions is
currently underway.
4.2. Kinetics of α → γ transformation on continuous heating
The second outcome of this study is concerned with the elucidation of
reaustenitisation reaction on heating. Admittedly, the formation of austenite from
tempered martensite microstructure is not a simple metallurgical phenomenon [53,
54]. It is clear that upon reaching Ac1, the lower critical temperature, both the
dissolution of carbide and the structural transformation of α-ferrite → austenite are
energetically feasible, but for kinetic factors, these concurrent reactions occur with
different velocities [55]. Of these, the structural transformation of (carbon lean) ferrite
to austenite is basically an interface diffusion-controlled process [55-57] while
carbide dissolution is a bulk or volume diffusion controlled phenomenon [27-29, 36].
The heterogeneous nucleation of austenite is catalysed by the presence of abundant
16. 16
internal interfaces to begin with, although at later stages, some other less potent
nucleation sites need to get activated [57]. Thus, in principle the nucleation rate of
austenite is one of continuously decreasing with time. However, assuming that
nucleation of austenite is adequately facilitated, the issue then is one of sustaining its
growth by enabling the transfer of atoms across the growing austenite/ferrite interface
[56]. From a mechanistic point of view, the austenite growth is possible even at a
higher heating rates, if it is mediated by the transfer of mobile species across the
growing γ/α interface [58].
In the case of carbide dissolution however, the steep concentration gradient
prevailing at the carbide/austenite or carbide/ferrite interfaces, both with respect to the
slow diffusing substitutional elements (Cr, Mo) and also to some extent with respect
to the relatively fast moving carbon atoms [36], dictates that volume diffusion in
austenite is the rate limiting one [36, 53, 54]. With this conceptual background the
role of heating rate in influencing the kinetics of carbide dissolution and hence
indirectly the austenitisation reaction is discussed next.
For very slow heating rates, the system can be assumed to evolve with the
possibility of realising local thermodynamic equilibrium with respect to mobile
carbon atoms at the interface. Under such circumstances, it is likely that the carbide
dissolution may get initiated even at relatively lower degree of superheating, that is
T>Ac1. The reaction proceeds to some extent, but certainly not to completion upon
reaching Ac3. The dissolution of carbides results in a gradual change in austenite
composition in the immediate vicinity and this affects subsequent austenite formation
kinetics in an indirect manner by effecting an increase in the activation energy for
carbon diffusion in austenite [40, 59].
17. 17
If on the contrary, the austenitisation is sought under relatively fast heating
conditions, the time scales provided are simply inadequate for the successful progress
of carbide dissolution [30]. Nevertheless, the ferrite to austenite structural change can
still be realised at these higher heating rates, with possibly a different mechanism, as
the work of Kaluba et al has demonstrated [58]. But even in such cases, it is highly
unlikely that transformation to austenite proceeds to 100 % completion upon reaching
Ac3. The presence of undissolved carbide particles may pin and retard the
advancement of γ/α interface. A slight superheating and or isothermal hold above Ac3
are often required to realise the complete formation of homogeneous austenite [20].
For intermediate heating rates, the actual picture is rather diffuse in the sense that both
carbide dissolution and α → γ phase change may proceed to different extents.
In terms of accounting for Qeff, it may be said that Qeff is reflective of the simple
interface diffusion controlled α → γ structural change under fast heating conditions.
However for slower heating rates, it is influenced certainly by the disintegration of the
carbide phase and its dissolution in the growing austenite phase. Judging the present
results in the light of the picture portrayed above, the gradual decrease in Q values
with increasing β can be rationalised. One final point is that the measured values of
Qeff is of the same order as that of the activation energy for chromium diffusion in the
austenite phase of a low alloy–low carbon steel (~ 260 kJ mol -1
)[59]. However, the
present estimate of Q is in direct contradiction to the normal value of about 110 – 120
kJ mol-1
quoted for austenitisation reaction in plain carbon or low alloy steels, wherein
the cementite or pearlite colony dissolution is more readily enabled. The higher values
of Qeff encountered in 9Cr-1Mo steels implies that simple carbon diffusion in austenite
model is not applicable for the α → γ reaction in highly alloyed power plant steels.
The experimental study of Lenel [27, 28] and the electron microscopy characterisation
18. 18
of austenite formation reaction in high chromium model alloys by Shtansky et al [29]
reinforce this viewpoint. It must be added that the understanding of the kinetics of
austenite formation and carbide dissolution in highly alloyed power plant and nuclear
grade steels is still far from complete and more studies need to be done to shed further
light onto this issue.
Conclusions
(i). A comprehensive differential scanning calorimetry characterisation of thermal
stability has been performed on four different varieties of mod. 9Cr-1Mo
welding consumables. Precise measurement of α → γ transformation
temperatures as a function of heating rate has also been made.
(ii). The transformation temperatures Ac1 and Ac3 are found to exhibit a strong
non-linear variation with heating rate, with the net effect of expanding the α+γ
two phase region to higher temperatures for higher rate of heating.
(iii). It is found that for nominally the same Cr/Mo content, the transformation
temperatures Ac1 and Ac3 exhibited a decrease with respect to increasing
(Mn+Ni) concentration. A high value of (Mn+Ni) content is also found to
record a lower enthalpy for the α-ferrite + carbide → γ -austenite, phase
change.
(iv). The kinetics of the α-ferrite + carbide → γ -austenite transformation has been
modelled after standard KJMA formalism and the apparent activation energy
for the overall phase change is estimated to be about 320-280 kJ mol-1
. The
activation energy is found to be sensitive to the heating rate; it decreased for
increasing rates of heating.
(v). For higher heating rates, it is suggested that the kinetics of α-ferrite + Carbide
→ γ -austenite transformation is found to be mainly interface controlled as no
19. 19
significant carbide dissolution is realised under such circumstance. For slow
heating, the accompanying M23C6 carbide dissolution in growing austenite
also makes an indirect contribution to overall activation energy.
Acknowledgements
The authors acknowledge sincerely the encouragement and sustained support
received from Dr. Baldev Raj, Dr. P. R. Vasudeva Rao and Dr. K. Bhanusankara Rao
during the course of this research. Shri. B. Jeya Ganesh acknowledges the award of
the junior research fellowship by DAE, India, as a part of which the present research
is carried out.
20. 20
References
1. F. Masuyama, ISIJ International, 241 (2001) 612-625.
2. R. K. Williams, R.S. Graves, F.J. Weaver and D. L. McElroy, The
Physical Properties of 9Cr1Mo steel from 300 to 1000 K, in: Proc. Of 17-
th International Thermal Conductivity conference, Gaithersburg, (1981).
3. V. K. Sikka, C. T. Ward and K. C. Thomas, Modified 9Cr-1Mo steel – An
improved alloy for steam generator applications, in: Ferritic Steels for
High-Temperature Applications, Ed. A. K. Khare, ASM, Metals Park,
OH, (1983), pp. 65-84.
4. F. Abe, M. Igarashi, N. Fujitsuna, K. Kimura and S. Muneki, Alloy design
of advanced ferritic steels for 650 0
C USC boilers, In : Conference
Proceeding on advanced heat resistant steel for power generation, San
Sebastian, Spain, Cambridge University Press, U.K (1988) p. 84 -97.
5. W. L. Bell, T. Lauritzen, and S. Vaidyanathan, Ferritics for breeder
reactor in-core applications: A survey of alloys, properties and
microstructure, in:,Topical Conference on ferritic alloys for use in nuclear
energy technologies, (eds.: J. W. Davis and D. J. Michel), ASM, Met. Soc.
AIME, Warrendale, PA (1983) pp. 113-124.
6. R.L. Klueh, K. Ehrlich and F. Abe, J. Nucl. Mater., 191-194 (1992) 116.
7. R. L. Klueh, Int. Mater. Rev., 50 (2005) 287.
8. Moriyasu Tokiwai, Masaki Horie, Kenji Kako and Masayuki Fujiwara, J.
Nucl. Mater., 204 (1993) 56.
9. M. Tamura, H. Hayakawa, M. Tamimura, A. Hishinuma and T. Kondo, J.
Nucl. Mater., 155-157 (1988) 620.
10. B. Van der Schaaf, D. S. Gelles, S. Jitsukawa, A. Kimura, R. L. Klueh, A.
Moslang and G. R Odette, J. Nucl. Mater., 283-287 (2000) 52.
11. S. Ukai, M. Harada, H. Okada, M. Inoue, S. Nomura, S. Shikakura, K.
Asabe, T. Nishida and M. Fujiwara, J. Nucl. Mater., 204 (1993) 65.
12. F. V. Ellis, J. F. Henry and B. W. Roberts, welding, Fabrication and
Service experience with modified 9Cr 1M0 steel, in : New Alloys for
Pressure vessels and Piping, PVP volume 201, American Society for
mechanical Engg., NY, (1990) pp. 55-63.
13. J. Onoro, Int. J. press. Vessels & piping, 83 (2006) 540-545.
14. R. G. Faulkner, J. A. Williams, E. Gonzalez-Sanchez, and A. W. Marshall,
Mater. Sci. Technol., 19 (2003) 347-354.
21. 21
15. F. B. Pickering, Physical Metallurgy and the Design of Steels, Applied
Science Publishers, London (1978).
16. R. J. Castro and J. J. Cadenet, Welding metallurgy of stainless and heat-
resisting steels, Cambridge university press, London, U.K. (1968).
17. AWS Welding Handbook, Vol. 4, Materials and Applications, 8th
ed.,
(1998).
18. S. J. Sanderson, Interrelationships between mechanical properties and
microstructure in a 9Cr 1Mo steel, in: Ferritic Steels for fast reactor steam
generators, BNES, London (1978), p.120.
19. S. K. Albert, C. R. Das and A. K. Bhaduri, Specifications for modified
9Cr-1Mo welding electrodes, IGCAR internal report, PFBR, 33010 SP
1006 (2002).
20. S. Raju, B. Jeya Ganesh, Aritra Banerjee and E. Mohandas, Mater. Sci.
Engg., A465 (2007) 29-37.
21. S. Raju, N. S. Arun Kumar, B. Jeyaganesh, E. Mohandas and U. Kamachi
Mudali, J. Alloys Compd., 440 (2007) 173-177.
22. B. Jeyaganesh, S. Raju, S. Murugesan, E. Mohandas and M.
Vijayalakshmi, Int. J. Thermophys., (2007), accepted for publication.
23. P. D. Desai, J. Phys. Chem. Ref. Data, 15 (1986) 967-972.
24. Q. Chen and B. Sundman, J. Phase Eq., 22 (2001) 631-644.
25. M. J. Richardson, in : K. D. Maglic, A. Cezairliyan, V. E. Peletsky (Eds.),
Compendium of Thermophysical Property Measurement Techniques, vol.
2, Plenum Press, New York, 1992, p.519.
26. A. Baltusnikas and R. Levinskas, Mater. Sci., 12 (2006) 192-198.
27. U. R. Lenel, Scripta Metall., 47 (1983) 471-474.
28. U. R. Lenel and R. W. K. Honeycombe, Metal. Sci., 18 (1984) 201-205.
29. D. V. Shtansky, K. Nakai and Y. Ohmori, Z. Metallkd., 90 (1999) 25-37.
30. A. Danon, C. Servant, A. Alamo, and J. C. Brachet, Mater. Sci. Engg., A
348 (2003) 122-132.
31. Bernhard C. Schaffernak and Hornst H. Cerjak, Calphad, 25 (2001) 241-
251.
32. A. Kroupa, J. Havrankova, M. Coufalava, M. Svoboda and J. Vrestal, J.
Phase Eq., 22 (2001) 312-323.
22. 22
33. A. Schneidner and G. Inden, Acta Mater., 53 (2005) 519-526.
34. J-O. Andersson, T. Helander, L. Hoglund, P. Shi and B. Sundman,
THERMOCALC &DICTRA, Computational tools for materials science,
Calphad, 26 (2002) 273-312.
35. V. A. Yardley and Y. de Carlan, J. Phase Equilibria. and Diffusion,
27(2006) 102-112.
36. A. Bjarbo and M. Hatterstrand, Mater. Trans., 32A (2001) 19-27.
37. J. Hald and L. Korcakova,. ISIJ Int., 43 (2003) 420-427.
38. B. Nath, E. Metcalfe, J. Hald, in : A. Strang, D. J. Gooch (Eds.),
Microstructural Development and Stability in high Chromium Ferritic
Steels, The institute of Materials, London, 1997, P. 123
39. Teresa M. V. R. de Barros, Rui. C. Santos, Anabela C. Fernandes and M.
E. Minas da Piedabe, Thermochim. Acta, 269/270 (1995) 51-60.
40. J. Miettinen, Metall and Mater. Trans., 28 B, (1997) 281-287.
41. A. Bodin and P. D. Marchal, Steel Res., 65 (1994) 103-109.
42. S. Raju, B. Jeyaganesh and E. Mohandas, unpublished research, (2007).
43. S. Vyazovkin, J. Thermal Analysis and Calor., 83 (2006) 45-51.
44. J. W. Christian, The theory of Transformations in Metals and Alloys, Part
I, Ch. 12, Pergamon Press, Oxford (1975).
45. G. Ruitenberg, E. Woldt and A. K. Petford-Long, Thermochim. Acta, 378
(2001) 97-105.
46. F. Liu, F. Sommer, and E.J. Mittemeijer, J. Mater. Sci., 39 (2004) 1621-
1634
47. M. J. Starink, Int. Mater. Rev., 49 (2004) 191-226.
48. F. C. Liu, F. Sommer and E. J. Mittemeijer, Acta Mater., 52 (2004) 2549-
2560.
49. E. Gamsjager, M. Militzer, F. Fazeli, J. Svoboda and F. D. Fischer, Comp.
Mat. Sci., 37 (2006) 94-100.
50. R. G. Thiessen, I. M. Richardson and J. Sietsma, Mater. Sci. Engg., A247
(2006) 225-231.
51. J. Onoro, J. Mater. Proc. Technology, 180 (2006) 137-142.
23. 23
52. V. Gaffard, A. F. Gourgues-Lorenzon and J. Besson, ISIJ Int., 45 (2005)
1015-1924.
53. R. Gullberg, J. Iron Steel Inst., 211 (1973) 59.
54. M. Hillert, K.Nilsson and L.E. Torndahl, J. Iron Steel Inst., 209, (1971)
49-66.
55. F. L. G. Oliveira, M. S. Andrade, A. B. Cota, Mater. Character.,58 (2007)
256-261.
56. R.C. Reed, T. Akbay, Z. Shen, J.M. Robinson, J.H. Root, Mater. Sci.
Engg., A256 (1998) 152-165.
57. W. Zhang, J. W. Elmer and T. Deb Roy, Scripta Mater., 46 (2002) 753-
757.
58. W.J. Kaluba, R. Taillard, and J. Foct, Acta mater., 46 (1998) 5917-5925.
59. Zs. Tokei, K. Hennessen, H. Viefhaus and H. J. Grabke, Mater. Sci. Tech.,
16 (2000) 1129.
60. J. Sietsma and S. Van der Zwaag, Acta mater., 52 (2004) 4143-4152.
24. 24
Table 1
Listing of the compositional details of mod. 9 Cr-1Mo welding consumables used in
this study. The composition is determined by direct reading optical emission
spectroscopy.
Elements Kobe
E9016
Boehler
E9016
Midhani
(E9016-B9)
Midhani
Filler Wire
Midhani
Base metal
( weight percent )
Carbon 0.06 0.075 0.1 0.084 0.097
Manganese 1.37 1.20 1 0.60 0.37
Silicon 0.30 0.30 0.24 0.30 0.31
Nickel 0.95 0.65 0.7 0.75 0.38
Phosphorous 0.005 0.008 0.009 0.007 0.018
Sulphur 0.001 0.007 0.012 0.0034 0. 0047
Chromium 9.24 9.3 9.0 8.89 9.29
Molybdenum 1.05 1.0 0.99 0.93 0.92
Niobium 0.03 0.009 0.05 0.08
Vanadium 0.17 0.23 0.17 0.22 0.26
Nitrogen 0.03 0.04 0.055 0.0375 0.057
Copper - - < 0.05 - -
Aluminium - - < 0.010 - -
Iron balance balance balance balance balance
Mn+ Ni 2.32 1.85 1.7 1.35 0.75
V+Nb 0.20 0.23 0.179 0.27 0.34
25. 25
Table 2
Listing of the Vickers microhardness values (VHN) for mod. 9Cr-1Mo welding
consumables. Italicised values are not considered for the final analysis.
Sample
description
Midhani
electrode
Kobe
electrode
Boehler
electrode
Base metal Midhani
Filler
1 503 473 503 339 560
2 514 493 483 336 572
3 514 488 498 339 560
4 514 488 503 322 542
5 514 488 483 342 548
6 514 488 464 351 519
Average 514 485 487 341 556
31. 31
Figure 1 (a-e) The optical micrographs of different electrode compositions : (a)
Boehler electrode, (b) Kobe electrode, (c) Midhani electrode, (d) Midhani filler, and
(e) base metal
e
32. 32
Figure 2. The room temperature x-ray diffraction profiles of different welding
consumables taken using Cu-Kα radiation.
20 40 60 80
(531)
(440)
(422)
a = 0.2875 nm
a = 0.2876 nm
a = 0.2876 nm
a = 0.2873 nm
M23
C6
carbide peak
Midhani : make E9016-B9
Kobe make : E 9016
Boehler make : E 9016
Midhani base metal
Mod. 9Cr1Mo Ferritic
Welding Consumables
αααα-(211)
αααα-(200)
αααα-(110)
Intensity(arbitraryunits)
2θθθθ (degrees)
35. 35
Figure 5. The fraction of austenite formed as a function of temperature for different
heating rates.
1040 1060 1080 1100 1120 1140 1160 1180
0.0
0.2
0.4
0.6
0.8
1.0
heating rate
increasing
9970504030201053
Mod. 9Cr 1Mo :
Weld consumable
Midhani electrode
(α - γ transformation)
Fractionofaustenite
Temperature (K)
36. 36
Figure 6 : The variation of Ac1 and Ac3 transformation temperatures with respect to
combined (Mn+Ni) content
0.8 1.2 1.6 2.0 2.4
900
950
1000
1050
1100
1150
Filler
Ac1
Ac3
K
obe
Boehler
Mod. 9Cr 1Mo welding consumables
M
idhani
M
idhani
Basemetal
Ac1
,Ac3
(K)
Mn + Ni (wt%)