EXPERIMENTAL STUDY ON THE BEHAVIOUR OF RETEMPERED CONCRETE K. Uma Shankar1, K. Arun Prakash2, M. Harshavardana Balaji3, S. Pradep Kumar4 1Assistant Professor, Department of Civil Engineering, Knowledge Institute of Technology, Kakkapalayam, Salem – 637 504, Tamil Nadu, India 2Assistant Professor, Department of Civil Engineering, Knowledge Institute of Technology, Kakkapalayam, Salem – 637 504, Tamil Nadu, India 3Assistant Professor, Department of Civil Engineering, Knowledge Institute of Technology, Kakkapalayam, Salem – 637 504, Tamil Nadu, India 4Assistant Professor, Department of Civil Engineering, Knowledge Institute of Technology, Kakkapalayam, Salem – 637 504, Tamil Nadu, India Abstract Ready–mixed concrete industries, are faced with a common problem known as casting delay, which usually results in a considerable loss of workability, so that concrete may be unworkable. On the other hand, improper methods of handling, lack of site organization, work scheduling and breakdown of equipment are some other causes of unexpected long delays. In such situations engineers at site, many a time reject the concrete partially set and unduly stiffened due to the time elapsed between mixing and placing. It is required to see whether such a stiffened concrete could be used on work without undue harm with use of admixtures. The process of remixing of concrete, if necessary, with addition of just the required quantity of water is known as “retempering” of concrete. The main objective of this research work is to study the behaviour and quality of retempered concrete and making it acceptable in concrete industry which would otherwise go as waste, thus saving the man hours, money and material. To achieve the above objective the workability, near surface characteristics and strength properties of retempered concrete at different time intervals such as, after 15 min, 30 min, 45 min, 60 min, 75 min, 90 min, 105 min and 120 min are found. Keywords: Retempering, workability, near surface characteristics, strength, behaviour, slump. 
---------------------------------------------------------------------***-------------------------------------------------------------------- 1. INTRODUCTION 
Concrete industries and, especially, ready-mixed concrete industries, are faced with a common problem known as casting delay, which usually results in a considerable loss of workability, so that concrete may be unworkable. Delay in the production and delivery of ready-mixed concrete is inevitable, which is influenced by the location of construction sites in relation to the central batching plant and traffic conditions on the route. On the other hand, improper methods of handling, lack of site organization, work scheduling and breakdown of equipment are some other causes of unexpected long delays. The practice of retempering is frequently performed to restore the initial slump and keep concrete workable at construction sites in order to cope with the need for expediting casting operations and reducing consolidation efforts. Retempering of concrete with water, superplasticizers or a combination of both, are the most common variants for resolving slump loss of concrete. However it is well-known that retempering with water alone results in a substantial strength loss, since extra water increases the water to cement ratio of the concrete mixture. In the case of ready-mixed concrete, when concrete is observed at the delivery point to have a lower-than- specified workability, there may be one or more of three possible reasons: (a) Insufficient water batched initially (b) a higher rate of evaporation (or)(absorption by aggregate) than anticipated and (c) a higher rate of hydration than expected. Based on established research, the retempering water added to offset reduction in workability, due to reasons (a) or (b), will not result in strength reduction, whereas extra water to combat (c) will result in a lower strength, due to some increase in the water to cement ratio. On the other hand, retempering with a superplasticizer would be beneficial in terms of the strength loss experienced [1]. 
One of the adverse effects of hot weather concreting is loss of slump. Delay in the delivery of ready mixed concrete has the same result and leads many people in the concrete industry to regain the original slump by adding water, a process known as 'retempering'. Ready-mixed (RMC) concrete, which is mixed at the plant, using a normal, well- designed concrete mix, should arrive at its destination with sufficient workability to enable it to be properly placed and fully compacted. In such circumstances, where there is a significant period of time between mixing and placing the concrete, there will be a noticeable reduction in the workability of the fresh concrete. If for any reason, the placement of the concrete is unduly delayed, then it may stiffen to an unacceptable degree and site staff would normally insist on the rejection of a batch or otherwise good concrete on the grounds of insufficient workability. If not rejected, excessive vibration would be needed to attempt to fully compact the concrete, with the risk of incomplete
IJRET: International Journal of Research in Engineering and Technology eISSN: 2319-1163 | pISSN: 2321-7308 
_______________________________________________________________________________________ 
Volume: 03 Special Issue: 11 | NCAMESHE - 2014 | Jun-2014, Available @ http://www.ijret.org 257 
compaction, expensive repair, or, at worst, removal of the hardened concrete. If abnormal slump loss in anticipated or if transport times are significant, then the intelligent use of admixtures can alleviate the potential workability difficulties, although at additional cost, and this practice is common place. However, in cases where unforeseen delay or some other cause has lead unexpectedly to poor workability, retempering of the concrete by water, while normally considered to be bad practice, may, in reality, be contemplated as a possible course of action. The increase in the water content of the concrete immediately prior to discharge will improve the consistency, but it is widely held that there must be a subsequent increase in the water / cement (w/c) ratio which will be detrimental to the hardened concrete. Adding water to a plastic mix to increase slump is an extremely common practice, even though it is not recommended because it increases the porosity of concrete. Concrete often arrives on site more than half an hour after initial mixing. Placement operations can take anywhere from 10 to 60 minutes, depending on the field conditions and the size of the load. When the slump decreases to an unacceptable level during the operations, water is added to the mix and, very often, experienced field inspectors will tolerate what can be termed 'reasonable' retempering, i.e., enough to increase slump by 50 or 60 mm [2]. 2. MATERIALS AND METHODOLOGY In this experimental work, ordinary Portland cement (OPC) 43 grade with cement content of 413.33 Kg /m3 conforming to IS: 8112 – 1989 [3] was used. Low calcium, class F dry fly ash from the silos of Raichur thermal power station conforming to IS: 3812 (Part 1) – 2003 [4] was used. Locally available river sand with specific gravity 2.58 belonging to zone II and locally available crushed angular aggregates of maximum nominal size 20mmwith specific gravity 2.61 were used confirming toIS: 383–1970 [5] and Water fit for drinking was used. 2.1 Methodology In this experimentation, the mix design was done as per IS: 10262 – 2009 [6] and the obtained mix proportion is 1:1.58:2.71 with W/C of 0.45. The quality of retempered concrete was checked w.r.t the following four different cases 
 Retempered concrete without any addition 
 Retempered concrete with extra 5% cement + extra 5% water 
 Retempered concrete with fly ash (20% replacement by cement) 
 Retempered concrete with fly ash (20% replacement by cement) and extra 5% cement +extra 5% water 
After thorough mixing of all the ingredients in dry state, the required quantity of water was added in the mix and thoroughly mixed. At this stage, the fresh concrete was kept for 15 minutes retempering time and thereafter workability tests were conducted, such as slump cone test, compaction factor test and Vee-Bee consistometer test. After conducting these tests the fresh concrete was poured into the moulds and the specimens were cast with sufficient compaction through tamping rod and vibrating table. This forms the retempered concrete for 15 minutes. Similarly the specimens were prepared with a retempering time of 30 minutes, 45 minutes, 60 minutes, 75 minutes, 90 minutes, 105 minutes and 120 minutes for all the above four combinations. All the specimens were demoulded after 24 hours of their casting and were transferred to curing tank to cure them for 28 days. After 28 days of curing the specimens were tested for the compressive strength, tensile strength, flexural strength and shear strength as per IS specifications. Near surface characteristic tests such as water absorption test and sorptivity tests were conducted to find percentage water absorption and sorptivity of retempered concrete. The sorptivity test determines the rate of capillary–rise absorption by a concrete cubes which rests on small supports in a manner such that only the lowest 30 mm of the cube is submerged. The increase in the water level of the prism with time is recorded. It has been shown that there exists a relation of the form, 
S = Where S = sorptivity in mm/min0.5. i = depth of water level increased by capillary action, expressed in mm. t = time measured in minutes at which the depth determined [7]. For compressive strength test, the cubes of size 150 x 150 x 150 mm were cast and tested under compression testing machine of 2000 kN capacity as per IS: 516-1959 [8]. For splitting tensile strength test, the cylinders of 150 mm diameter and length 300 mm were cast and were tested under compression testing machine as per IS: 5816-1999 [9]. For flexural strength test, beams of dimension 100 x 100 x 500 mm were cast and were tested on an effective span of 400 mm with two point loading as per IS: 516-1959 [8]. For shear strength test L shaped specimens as shown in fig. 1 were used.
IJRET: International Journal of Research in Engineering and Technology eISSN: 2319-1163 | pISSN: 2321-7308 
_______________________________________________________________________________________ 
Volume: 03 Special Issue: 11 | NCAMESHE - 2014 | Jun-2014, Available @ http://www.ijret.org 258 
Fig.1 Shear test on L shaped specimen The specimen was centrally placed on the compression testing machine and load is applied continuously and uniformly. The load is increased until the specimen fails and record the maximum load carried by each specimen during the test. Computation of the shear strength was done as follows. 
Failure load = 
Shear strength = 
× 1000 
Where, P = Load in kN A = Area of shear surface = 60 x 150 mm2 L1 = 25 mm L2 = 25 mm. 3.0 RESULTS AND DISCUSSIONS Table 1 gives the slump test results of different retempered concrete combinations for different retempering times, and fig. 2 shows the variation of slump. Table 2 gives the compaction factor test results of different retempered concrete combinations for different retempering times, and fig. 3 shows the variation of compaction factor. Table 3 gives the Vee–Bee test results of different retempered concrete combinations for different retempering times, and fig. 4 shows the variation of Vee–Bee time. 
Table 1: Slump test results 
Slump (mm) of retempered concrete 
Retempering time 
without any 
with extra 5% 
with fly ash (20% 
with fly ash (20% replacement 
(minutes) 
cement + extra 5% 
replacement by 
by cement) and extra 5% 
additions 
water 
cement) 
cement + extra 5% water 
0 
10 
15 
20 
25 
15 
10 
15 
20 
25 
30 
10 
15 
20 
25 
45 
8 
12 
15 
25 
60 
8 
12 
15 
20 
75 
5 
10 
12 
20 
90 
5 
8 
10 
15 
105 
4 
5 
8 
10 
120 
0 
3 
4 
5 
Table 2: Compaction factor test results 
Compaction factor of retempered concrete 
Retempering time 
without any 
with extra 5% 
with fly ash (20% 
with fly ash (20% replacement 
(minutes) 
cement + extra 5% 
replacement by 
by cement) and extra 5% 
additions 
water 
cement) 
cement + extra 5% water
IJRET: International Journal of Research in Engineering and Technology eISSN: 2319-1163 | pISSN: 2321-7308 
_______________________________________________________________________________________ 
Volume: 03 Special Issue: 11 | NCAMESHE - 2014 | Jun-2014, Available @ http://www.ijret.org 259 
0 
0.865 
0.869 
0.882 
0.896 
15 
0.862 
0.868 
0.876 
0.893 
30 
0.860 
0.868 
0.875 
0.885 
45 
0.858 
0.866 
0.873 
0.880 
60 
0.857 
0.861 
0.865 
0.871 
75 
0.851 
0.859 
0.861 
0.865 
90 
0.847 
0.854 
0.858 
0.863 
105 
0.845 
0.851 
0.855 
0.858 
120 
0.844 
0.848 
0.852 
0.853 
Table 3: Vee–Bee test results 
Vee Bee time (sec) of retempered concrete 
Retempering time (minutes) 
without any additions 
with extra 5% 
with fly ash (20% 
with fly ash (20% replacement 
cement + extra 5% 
replacement by 
by cement) and extra 5% 
water 
cement) 
cement + extra 5% water 
0 
5 
4 
3 
2 
15 
5 
4 
3 
2 
30 
6 
5 
3 
2 
45 
6 
5 
4 
2 
60 
6 
5 
4 
3 
75 
7 
6 
4 
3 
90 
8 
6 
5 
3 
105 
8 
7 
5 
4 
120 
8 
7 
5 
4 
Fig. 2 Variation of slump Fig. 3 Variation of compaction factor
IJRET: International Journal of Research in Engineering and Technology eISSN: 2319-1163 | pISSN: 2321-7308 
_______________________________________________________________________________________ 
Volume: 03 Special Issue: 11 | NCAMESHE - 2014 | Jun-2014, Available @ http://www.ijret.org 260 
Fig. 4 Variation of Vee–Bee time 
It is observed that workability as measured from slump, compaction factor and Vee–Bee degree go on decreasing as the retempering time increase. This is true for retempered concrete produced without any additions, produced with extra 5% cement and water, produced with 20% replacement of cement by fly ash, and produced with 20% replacement of cement by fly ash with extra 5% cement and water. This is due to the fact that as the retempering time increases the evaporation of water takes place from the concrete mass and also concrete starts losing its plasticity, thereby reducing workability. Thus it can be concluded that the workability goes on decreasing as the retempering time increase. Also it is observed that workability as measured from slump, compaction factor and Vee–Bee degree is more for the retempered concrete produced with 20% replacement of cement by fly ash and with extra 5% cement and water as compared to other categories. Thisis true for all the retempering times.This is due to the fact that addition of fly ash and extra 5% cement and water will help in keeping the concrete in plastic state for more time thus inducing the flow characteristics.Thus it can be concluded that the workability of retempered concrete produced with 20% replacement of cement by fly ash with extra 5% cement and water is high as compared to other categories of retempered concrete. 
Table 4 gives the water absorption test results of different retempered concrete combinations for different retempering times, and fig. 5 shows the variation of water absorption. Table 5 gives the sorptivity test results of different retempered concrete combinations for different retempering times, and fig. 6 shows the variation of sorptivity. Table 4: Water absorption test results 
Water absorption (%) of retempered concrete 
Retempering time (minutes) 
without any 
with extra 5% 
with fly ash (20% 
with fly ash (20% replacement 
cement + extra 5% 
replacement by 
by cement) and extra 5% 
additions 
water 
cement) 
cement + extra 5% water 
0 
0.800 
0.776 
0.742 
0.735 
15 
0.853 
0.805 
0.793 
0.746 
30 
0.860 
0.835 
0.821 
0.770 
45 
0.928 
0.875 
0.843 
0.790 
60 
0.937 
0.899 
0.851 
0.849 
75 
0.955 
0.939 
0.867 
0.864 
90 
0.985 
0.953 
0.921 
0.901 
105 
1.002 
0.968 
0.928 
0.923 
120 
1.058 
0.991 
0.944 
0.942 
Table 5: Sorptivity test results 
Sorptivity (mm/min0.5) of retempered concrete 
without any 
with extra 5% 
with fly ash (20% 
with fly ash (20% replacement 
(minutes) 
cement + extra 5% 
replacement by 
by cement) and extra 5% 
additions 
water 
cement) 
cement + extra 5% water 
0 
4.52 
4.39 
4.00 
3.87 
15 
4.65 
4.52 
4.13 
4.00
IJRET: International Journal of Research in Engineering and Technology eISSN: 2319-1163 | pISSN: 2321-7308 
_______________________________________________________________________________________ 
Volume: 03 Special Issue: 11 | NCAMESHE - 2014 | Jun-2014, Available @ http://www.ijret.org 261 
30 
4.78 
4.65 
4.26 
4.13 
45 
4.78 
4.65 
4.26 
4.13 
60 
4.91 
4.65 
4.26 
4.13 
75 
4.91 
4.78 
4.39 
4.26 
90 
5.03 
4.91 
4.52 
4.39 
105 
5.29 
5.03 
4.78 
4.52 
120 
5.42 
5.16 
4.91 
4.65 
Fig. 5 Variation of water absorption Fig. 6 Variation of sorptivity 
It is observed that near surface characteristics as measured from water absorption and sorptivity go on increasing as the retempering time increase. This is true for retempered concrete produced without any additions, produced with extra 5% cement and water, produced with 20% replacement of cement by fly ash, and produced with 20% replacement of cement by fly ash with extra 5% cement and water. This is due to the fact that as the retempering time increases the workability decreases. This results in improper compaction of concrete which may lead to many air– voids in the concrete mass, thereby increasing water absorption and sorptivity.Thus it can be concluded that the near surface characteristics such as water absorption and sorptivity goes on increasing as the retempering time increase. 
Also it is observed that near surface characteristics as measured from water absorption and sorptivity is least for retempered concrete produced with 20% replacement of cement by fly ash with extra 5% cement and water as compared to other categories. This is true for all the retempering times. This is due to the fact that addition of fly ash with extra 5% cement and water induce plasticity to concrete resulting in more workability. This concrete can be easily compacted thereby reducing the air voids. Thus it can be concluded that the near surface characteristics such as water absorption and sorptivity is least for retempered concrete produced with 20% replacement of cement by fly ash with extra 5% cement and water as compared to other categories of retempered concrete. 
Table 6 gives the results of compressive strength of retempered concrete for different combinations with different retempering times, and fig. 7 shows the variation of compressive strength. Table 7 gives the results of tensile strength of retempered concrete for different combinations with different retempering times, and fig. 8 shows the variation of tensile strength. Table 8 gives the results of flexural strength of retempered concrete for different combinations with different retempering times, and fig. 9 shows the variation of flexural strength. Table 9 gives the results of shear strength of retempered concrete for different combinations with different retempering times, and fig. 10 shows the variation of shear strength. 
Table 6: Results of compressive strength 
Compressive strength (MPa) of retempered concrete 
Retempering time 
with extra 5% 
with fly ash 
with fly ash (20% 
without any 
replacement by cement) and 
(minutes) 
cement + extra 5% 
(20% replacement 
additions 
extra 5% cement + extra 5% 
water 
by cement)
IJRET: International Journal of Research in Engineering and Technology eISSN: 2319-1163 | pISSN: 2321-7308 
_______________________________________________________________________________________ 
Volume: 03 Special Issue: 11 | NCAMESHE - 2014 | Jun-2014, Available @ http://www.ijret.org 262 
water 
0 
42.22 
42.37 
42.67 
43.11 
15 
42.81 
43.26 
43.41 
43.56 
30 
43.11 
43.70 
43.85 
44.15 
45 
43.41 
44.15 
44.44 
44.89 
60 
42.37 
42.96 
43.11 
43.41 
75 
41.48 
42.07 
42.37 
42.67 
90 
40.74 
41.33 
41.63 
41.78 
105 
40.00 
40.15 
40.44 
40.74 
120 
39.11 
39.26 
39.56 
40.30 
Table 7: Results of tensile strength 
Tensile strength (MPa) of retempered concrete 
Retempering time 
with extra 5% 
with fly ash 
with fly ash (20% 
without any 
replacement by cement) 
(minutes) 
cement + extra 
(20% replacement 
additions 
and extra 5% cement + 
5% water 
by cement) 
extra 5% water 
0 
3.68 
3.77 
3.82 
3.91 
15 
3.77 
3.87 
3.96 
4.10 
30 
3.87 
3.96 
4.10 
4.20 
45 
3.96 
4.15 
4.29 
4.39 
60 
3.87 
4.01 
4.10 
4.20 
75 
3.68 
3.87 
3.91 
3.96 
90 
3.58 
3.68 
3.72 
3.82 
105 
3.44 
3.49 
3.54 
3.63 
120 
3.30 
3.39 
3.44 
3.54 
Table 8: Results of flexural strength 
Flexural strength (MPa) of retempered concrete 
Retempering time 
with extra 5% 
with fly ash 
with fly ash (20% 
without any 
replacement by cement) 
(minutes) 
cement + extra 
(20% replacement 
additions 
and extra 5% cement + 
5% water 
by cement) 
extra 5% water 
0 
6.47 
6.80 
7.13 
7.40 
15 
6.93 
7.20 
7.40 
7.67 
30 
7.20 
7.47 
7.93 
8.07 
45 
7.73 
7.87 
8.27 
8.73 
60 
6.80 
7.20 
7.47 
7.87 
75 
6.47 
6.80 
7.20 
7.60 
90 
6.07 
6.47 
6.80 
7.33 
105 
5.67 
6.13 
6.53 
6.80 
120 
5.47 
5.80 
6.33 
6.60
IJRET: International Journal of Research in Engineering and Technology eISSN: 2319-1163 | pISSN: 2321-7308 
_______________________________________________________________________________________ 
Volume: 03 Special Issue: 11 | NCAMESHE - 2014 | Jun-2014, Available @ http://www.ijret.org 263 
Table 9: Results of shear strength 
Shear strength (MPa) of retempered concrete 
Retempering time 
with extra 5% 
with fly ash 
with fly ash (20% 
without any 
replacement by cement) 
(minutes) 
cement + extra 
(20% replacement 
additions 
and extra 5% cement + 
5% water 
by cement) 
extra 5% water 
0 
3.70 
4.07 
4.26 
4.44 
15 
4.07 
4.26 
4.44 
4.63 
30 
4.26 
4.63 
4.81 
5.00 
45 
4.63 
4.81 
5.19 
5.37 
60 
4.44 
4.63 
4.81 
5.00 
75 
3.89 
4.07 
4.44 
4.81 
90 
3.52 
3.70 
4.07 
4.44 
105 
3.15 
3.33 
3.70 
4.07 
120 
2.96 
3.15 
3.33 
3.70 
Fig. 7 Variation of compressive strength Fig. 9 Variation of flexural strength 
Fig. 8 Variation of tensile strength Fig. 10 Variation of shear strength
IJRET: International Journal of Research in Engineering and Technology eISSN: 2319-1163 | pISSN: 2321-7308 
_______________________________________________________________________________________ 
Volume: 03 Special Issue: 11 | NCAMESHE - 2014 | Jun-2014, Available @ http://www.ijret.org 264 
It is observed that compressive strength, tensile strength, flexural strength and shear strength of retempered concrete goes on increasing up to 45 minutes of retempering time. Thereafter all the strengths start decreasing. This is true for retempered concrete produced without any additions, produced with extra 5% cement and water, produced with 20% replacement of cement by fly ash, and produced with 20% replacement of cement by fly ash with extra 5% cement and water. This is due to the fact that above 45 minutes of retempering time the concrete looses the plasticity seriously and remixing the concrete beyond 45 minutes will not reunite the concrete particles to adhere together. Thus it can be concluded that compressive strength, tensile strength, flexural strength and shear strength of retempered concrete goes on increasing up to 45 minutes of retempering time. Therefore retempering can be allowed up to 45 minutes. Also it is observed that compressive strength, tensile strength, flexural strength and shear strength of concrete is more for retempered concrete produced with 20% replacement of cement by fly ash with extra 5% cement and water as compared to other categories. This is true for all the retempering times. This is due to the fact that addition of fly ash and extra 5% cement and water will help in keeping the concrete in plastic state which helps in thorough compaction of concrete resulting in higher strength.Thus it can be concluded that compressive strength, tensile strength, flexural strength and shear strength of concrete is more for retempered concrete produced with 20% replacement of cement by fly ash with extra 5% cement and water as compared to other categories. 4. CONCLUSIONS Following conclusions can be drawn based on the experimentations conducted on the retempered concrete. 
 Workability goes on decreasing as the retempering time increase. 
 Workability of retempered concrete produced with 20% replacement of cement by fly ash with extra 5% cement and water is high as compared to other categories of retempered concrete. 
 Near surface characteristics such as water absorption and sorptivity goes on increasing as the retempering time increase. 
 Near surface characteristics such as water absorption and sorptivity is least for retemperedconcrete produced with 20% replacement of cement by fly ash with extra 5% cement and water as compared to other categories of retempered concrete. 
 Compressive strength, tensile strength, flexural strength and shear strength of retemperedconcrete goes on increasing up to 45 minutes of retempering time. Therefore retempering can be allowed up to the time of 45 minutes. 
 Compressive strength, tensile strength, flexural strength and shear strength of concrete is more for retempered concrete produced with 20% replacement of cement by fly ash with extra 5% cement and water as compared to other categories. 
REFERENCES 
[1]. IS: 8112 – 1989, ―43 Grade ordinary Portland cement—Specifications‖ (First revision),BIS, New Delhi, May 1990. 
[2]. IS: 3812 (Part 1) – 2003, ―Pulverized fuel ash – Specification‖ (Second revision),BIS, New Delhi, October 2003. 
[3]. IS: 383 – 1970, ―Specifications for coarse and fine aggregate from natural sources for concrete‖ (Second revision), BIS, New Delhi, April 1971. 
[4]. IS: 10262 – 2009, ―Concrete mix proportioning – Guidelines‖ (First revision), BIS, New Delhi, July 2009. 
[5]. IS: 10262-1982 Recommended Guidelines for Concrete Mix Design. 
[6]. SANTHAKUMAR.A.R,―Concrete Technology‖, Oxford Publishing & Co., New Delhi, 2007, First Edition. 
BIOGRAPHIES 
Prof.K.UmaShankar presently working as Assistant Professor in the department of Civil Engineering at Knowledge Institute of Technology. He has more than 4 years of teaching experience. He has published 5 papers in the reputed International and National journals & Conferences. 
Mr.K.ArunPrakash is presently working as Assistant Professor in the Department of Civil Engineering at Knowledge Institute of Technology. He has more than 3 years of teaching experience. He has published 1 paper in the International Conference and 2 papers in the National Conferences. 
Mr.M.Harshavardana Balaji is presently working as Assistant Professor in the Department of Civil Engineering at Knowledge Institute of Technology. He has more than 2 years of teaching experience. He has published 1 paper in the International Conference and 2 papers in the National Conferences. 
S.PradeepKumar is presently working as Assistant Professor in the Department of Civil Engineering at Knowledge Institute of Technology. He has more than 2 years of teaching experience. He has published 1 paper in the International Conference and 2 papers in the National Conferences.

More Related Content

What's hot

Effect of Ground Granulated Blast Furnace Slag as Partial Cement Replacement ...
Effect of Ground Granulated Blast Furnace Slag as Partial Cement Replacement ...Effect of Ground Granulated Blast Furnace Slag as Partial Cement Replacement ...
Effect of Ground Granulated Blast Furnace Slag as Partial Cement Replacement ...IRJET Journal
 
Use of Quarry Dust as Fine Aggregates by Partial Replacement of Sand in Conc...
Use of Quarry Dust as Fine Aggregates by Partial Replacement of  Sand in Conc...Use of Quarry Dust as Fine Aggregates by Partial Replacement of  Sand in Conc...
Use of Quarry Dust as Fine Aggregates by Partial Replacement of Sand in Conc...IRJET Journal
 
IRJET- Effect on M30 SCBA Concrete in Acidic Environment
IRJET-  	  Effect on M30 SCBA Concrete in Acidic EnvironmentIRJET-  	  Effect on M30 SCBA Concrete in Acidic Environment
IRJET- Effect on M30 SCBA Concrete in Acidic EnvironmentIRJET Journal
 
Membrane Distillation Review and Flux prediction in Direct Contact Membrane D...
Membrane Distillation Review and Flux prediction in Direct Contact Membrane D...Membrane Distillation Review and Flux prediction in Direct Contact Membrane D...
Membrane Distillation Review and Flux prediction in Direct Contact Membrane D...IRJET Journal
 
Fresh and Hardened Properties of Ground Granulated Blast Furnace Slag Made Co...
Fresh and Hardened Properties of Ground Granulated Blast Furnace Slag Made Co...Fresh and Hardened Properties of Ground Granulated Blast Furnace Slag Made Co...
Fresh and Hardened Properties of Ground Granulated Blast Furnace Slag Made Co...IJMREMJournal
 
Flow time analysis of blended mixes using Marsh cone apparatus
Flow time analysis of blended mixes using Marsh cone apparatusFlow time analysis of blended mixes using Marsh cone apparatus
Flow time analysis of blended mixes using Marsh cone apparatusAbdulRazakBH
 
IRJET- Self Compacting Concrete with Replacement of Flyash Aggregate as Fine ...
IRJET- Self Compacting Concrete with Replacement of Flyash Aggregate as Fine ...IRJET- Self Compacting Concrete with Replacement of Flyash Aggregate as Fine ...
IRJET- Self Compacting Concrete with Replacement of Flyash Aggregate as Fine ...IRJET Journal
 
IRJET- High Performance Concrete by using M Sand with Admixture 300
IRJET- High Performance Concrete by using M Sand with Admixture 300IRJET- High Performance Concrete by using M Sand with Admixture 300
IRJET- High Performance Concrete by using M Sand with Admixture 300IRJET Journal
 
Project Report on Concrete Mix Design of Grade M35
Project Report on Concrete Mix Design of Grade M35Project Report on Concrete Mix Design of Grade M35
Project Report on Concrete Mix Design of Grade M35Gyan Prakash
 
EFFECT OF RECRON FIBRES ON FLEXURAL BEHAVIOR ON CONCRETE
EFFECT OF RECRON FIBRES ON FLEXURAL BEHAVIOR ON CONCRETEEFFECT OF RECRON FIBRES ON FLEXURAL BEHAVIOR ON CONCRETE
EFFECT OF RECRON FIBRES ON FLEXURAL BEHAVIOR ON CONCRETES.m. Kumar
 
An experimental study on durability and water absorption properties of pervio...
An experimental study on durability and water absorption properties of pervio...An experimental study on durability and water absorption properties of pervio...
An experimental study on durability and water absorption properties of pervio...eSAT Journals
 
An experimental study on durability and water absorption properties of pervio...
An experimental study on durability and water absorption properties of pervio...An experimental study on durability and water absorption properties of pervio...
An experimental study on durability and water absorption properties of pervio...eSAT Publishing House
 
IRJET- Parametric Optimization of the Surface Characteristics of Rock Dus...
IRJET-  	  Parametric Optimization of the Surface Characteristics of Rock Dus...IRJET-  	  Parametric Optimization of the Surface Characteristics of Rock Dus...
IRJET- Parametric Optimization of the Surface Characteristics of Rock Dus...IRJET Journal
 
A Study on Strength Properties of Concrete Made with Waste Ready-Mix Concrete...
A Study on Strength Properties of Concrete Made with Waste Ready-Mix Concrete...A Study on Strength Properties of Concrete Made with Waste Ready-Mix Concrete...
A Study on Strength Properties of Concrete Made with Waste Ready-Mix Concrete...IRJET Journal
 
Self Consolidating Concrete-Designing & Tsting
Self Consolidating Concrete-Designing & TstingSelf Consolidating Concrete-Designing & Tsting
Self Consolidating Concrete-Designing & TstingJeewapriya Alahakoon
 

What's hot (20)

Effect of Ground Granulated Blast Furnace Slag as Partial Cement Replacement ...
Effect of Ground Granulated Blast Furnace Slag as Partial Cement Replacement ...Effect of Ground Granulated Blast Furnace Slag as Partial Cement Replacement ...
Effect of Ground Granulated Blast Furnace Slag as Partial Cement Replacement ...
 
J48077280
J48077280J48077280
J48077280
 
Use of Quarry Dust as Fine Aggregates by Partial Replacement of Sand in Conc...
Use of Quarry Dust as Fine Aggregates by Partial Replacement of  Sand in Conc...Use of Quarry Dust as Fine Aggregates by Partial Replacement of  Sand in Conc...
Use of Quarry Dust as Fine Aggregates by Partial Replacement of Sand in Conc...
 
IRJET- Effect on M30 SCBA Concrete in Acidic Environment
IRJET-  	  Effect on M30 SCBA Concrete in Acidic EnvironmentIRJET-  	  Effect on M30 SCBA Concrete in Acidic Environment
IRJET- Effect on M30 SCBA Concrete in Acidic Environment
 
Membrane Distillation Review and Flux prediction in Direct Contact Membrane D...
Membrane Distillation Review and Flux prediction in Direct Contact Membrane D...Membrane Distillation Review and Flux prediction in Direct Contact Membrane D...
Membrane Distillation Review and Flux prediction in Direct Contact Membrane D...
 
Fresh and Hardened Properties of Ground Granulated Blast Furnace Slag Made Co...
Fresh and Hardened Properties of Ground Granulated Blast Furnace Slag Made Co...Fresh and Hardened Properties of Ground Granulated Blast Furnace Slag Made Co...
Fresh and Hardened Properties of Ground Granulated Blast Furnace Slag Made Co...
 
Flow time analysis of blended mixes using Marsh cone apparatus
Flow time analysis of blended mixes using Marsh cone apparatusFlow time analysis of blended mixes using Marsh cone apparatus
Flow time analysis of blended mixes using Marsh cone apparatus
 
IRJET- Self Compacting Concrete with Replacement of Flyash Aggregate as Fine ...
IRJET- Self Compacting Concrete with Replacement of Flyash Aggregate as Fine ...IRJET- Self Compacting Concrete with Replacement of Flyash Aggregate as Fine ...
IRJET- Self Compacting Concrete with Replacement of Flyash Aggregate as Fine ...
 
IRJET- High Performance Concrete by using M Sand with Admixture 300
IRJET- High Performance Concrete by using M Sand with Admixture 300IRJET- High Performance Concrete by using M Sand with Admixture 300
IRJET- High Performance Concrete by using M Sand with Admixture 300
 
Project Report on Concrete Mix Design of Grade M35
Project Report on Concrete Mix Design of Grade M35Project Report on Concrete Mix Design of Grade M35
Project Report on Concrete Mix Design of Grade M35
 
EFFECT OF RECRON FIBRES ON FLEXURAL BEHAVIOR ON CONCRETE
EFFECT OF RECRON FIBRES ON FLEXURAL BEHAVIOR ON CONCRETEEFFECT OF RECRON FIBRES ON FLEXURAL BEHAVIOR ON CONCRETE
EFFECT OF RECRON FIBRES ON FLEXURAL BEHAVIOR ON CONCRETE
 
An experimental study on durability and water absorption properties of pervio...
An experimental study on durability and water absorption properties of pervio...An experimental study on durability and water absorption properties of pervio...
An experimental study on durability and water absorption properties of pervio...
 
An experimental study on durability and water absorption properties of pervio...
An experimental study on durability and water absorption properties of pervio...An experimental study on durability and water absorption properties of pervio...
An experimental study on durability and water absorption properties of pervio...
 
IRJET- Parametric Optimization of the Surface Characteristics of Rock Dus...
IRJET-  	  Parametric Optimization of the Surface Characteristics of Rock Dus...IRJET-  	  Parametric Optimization of the Surface Characteristics of Rock Dus...
IRJET- Parametric Optimization of the Surface Characteristics of Rock Dus...
 
A Study on Strength Properties of Concrete Made with Waste Ready-Mix Concrete...
A Study on Strength Properties of Concrete Made with Waste Ready-Mix Concrete...A Study on Strength Properties of Concrete Made with Waste Ready-Mix Concrete...
A Study on Strength Properties of Concrete Made with Waste Ready-Mix Concrete...
 
Self Consolidating Concrete-Designing & Tsting
Self Consolidating Concrete-Designing & TstingSelf Consolidating Concrete-Designing & Tsting
Self Consolidating Concrete-Designing & Tsting
 
20320140503015
2032014050301520320140503015
20320140503015
 
458
458458
458
 
Main projor
Main projor Main projor
Main projor
 
report work
report workreport work
report work
 

Viewers also liked

Design and development of non server peer 2 peer secure communication using j...
Design and development of non server peer 2 peer secure communication using j...Design and development of non server peer 2 peer secure communication using j...
Design and development of non server peer 2 peer secure communication using j...eSAT Publishing House
 
Performance evaluation of ti n coated carbide insert
Performance evaluation of ti n coated carbide insertPerformance evaluation of ti n coated carbide insert
Performance evaluation of ti n coated carbide inserteSAT Publishing House
 
Survey on securing outsourced storages in cloud
Survey on securing outsourced storages in cloudSurvey on securing outsourced storages in cloud
Survey on securing outsourced storages in cloudeSAT Publishing House
 
Comparative analysis of edge based and region based active contour using leve...
Comparative analysis of edge based and region based active contour using leve...Comparative analysis of edge based and region based active contour using leve...
Comparative analysis of edge based and region based active contour using leve...eSAT Publishing House
 
Application of dual tone multi frequency technology
Application of dual tone multi frequency technologyApplication of dual tone multi frequency technology
Application of dual tone multi frequency technologyeSAT Publishing House
 
Generalized fryze control strategy for shunt and
Generalized fryze control strategy for shunt andGeneralized fryze control strategy for shunt and
Generalized fryze control strategy for shunt andeSAT Publishing House
 
Simulation of collision avoidance by navigation
Simulation of collision avoidance by navigationSimulation of collision avoidance by navigation
Simulation of collision avoidance by navigationeSAT Publishing House
 
Analysis of roucairol and carvalho approach in
Analysis of roucairol and carvalho approach inAnalysis of roucairol and carvalho approach in
Analysis of roucairol and carvalho approach ineSAT Publishing House
 
The heating pattern of the microwave dehydrator for treating petroleum crude ...
The heating pattern of the microwave dehydrator for treating petroleum crude ...The heating pattern of the microwave dehydrator for treating petroleum crude ...
The heating pattern of the microwave dehydrator for treating petroleum crude ...eSAT Publishing House
 
Throughput analysis of energy aware routing protocol
Throughput analysis of energy aware routing protocolThroughput analysis of energy aware routing protocol
Throughput analysis of energy aware routing protocoleSAT Publishing House
 
Measuring effort for modifying software package as
Measuring effort for modifying software package asMeasuring effort for modifying software package as
Measuring effort for modifying software package aseSAT Publishing House
 
Control of inverters to support bidirectional power flow in grid connected sy...
Control of inverters to support bidirectional power flow in grid connected sy...Control of inverters to support bidirectional power flow in grid connected sy...
Control of inverters to support bidirectional power flow in grid connected sy...eSAT Publishing House
 
An efficient monitoring system for sports person using wi fi communication
An efficient monitoring system for sports person using wi fi communicationAn efficient monitoring system for sports person using wi fi communication
An efficient monitoring system for sports person using wi fi communicationeSAT Publishing House
 
Quality analysis of drinking water in bhopal city
Quality analysis of drinking water in bhopal cityQuality analysis of drinking water in bhopal city
Quality analysis of drinking water in bhopal cityeSAT Publishing House
 
Thermodynamic behavior of tetrahydrofuron in p dioxane, methylcyclohexane and...
Thermodynamic behavior of tetrahydrofuron in p dioxane, methylcyclohexane and...Thermodynamic behavior of tetrahydrofuron in p dioxane, methylcyclohexane and...
Thermodynamic behavior of tetrahydrofuron in p dioxane, methylcyclohexane and...eSAT Publishing House
 
Conception of a water level detector (tide gauge) based on a electromagnetic ...
Conception of a water level detector (tide gauge) based on a electromagnetic ...Conception of a water level detector (tide gauge) based on a electromagnetic ...
Conception of a water level detector (tide gauge) based on a electromagnetic ...eSAT Publishing House
 
Prediction of tool wear during turning of en9 work material against coated ca...
Prediction of tool wear during turning of en9 work material against coated ca...Prediction of tool wear during turning of en9 work material against coated ca...
Prediction of tool wear during turning of en9 work material against coated ca...eSAT Publishing House
 
Can fracture mechanics predict damage due disaster of structures
Can fracture mechanics predict damage due disaster of structuresCan fracture mechanics predict damage due disaster of structures
Can fracture mechanics predict damage due disaster of structureseSAT Publishing House
 
Cyclone disaster on housing and coastal area
Cyclone disaster on housing and coastal areaCyclone disaster on housing and coastal area
Cyclone disaster on housing and coastal areaeSAT Publishing House
 
Modeling of laminar flow tubular reactor using velocity profile
Modeling of laminar flow tubular reactor using velocity profileModeling of laminar flow tubular reactor using velocity profile
Modeling of laminar flow tubular reactor using velocity profileeSAT Publishing House
 

Viewers also liked (20)

Design and development of non server peer 2 peer secure communication using j...
Design and development of non server peer 2 peer secure communication using j...Design and development of non server peer 2 peer secure communication using j...
Design and development of non server peer 2 peer secure communication using j...
 
Performance evaluation of ti n coated carbide insert
Performance evaluation of ti n coated carbide insertPerformance evaluation of ti n coated carbide insert
Performance evaluation of ti n coated carbide insert
 
Survey on securing outsourced storages in cloud
Survey on securing outsourced storages in cloudSurvey on securing outsourced storages in cloud
Survey on securing outsourced storages in cloud
 
Comparative analysis of edge based and region based active contour using leve...
Comparative analysis of edge based and region based active contour using leve...Comparative analysis of edge based and region based active contour using leve...
Comparative analysis of edge based and region based active contour using leve...
 
Application of dual tone multi frequency technology
Application of dual tone multi frequency technologyApplication of dual tone multi frequency technology
Application of dual tone multi frequency technology
 
Generalized fryze control strategy for shunt and
Generalized fryze control strategy for shunt andGeneralized fryze control strategy for shunt and
Generalized fryze control strategy for shunt and
 
Simulation of collision avoidance by navigation
Simulation of collision avoidance by navigationSimulation of collision avoidance by navigation
Simulation of collision avoidance by navigation
 
Analysis of roucairol and carvalho approach in
Analysis of roucairol and carvalho approach inAnalysis of roucairol and carvalho approach in
Analysis of roucairol and carvalho approach in
 
The heating pattern of the microwave dehydrator for treating petroleum crude ...
The heating pattern of the microwave dehydrator for treating petroleum crude ...The heating pattern of the microwave dehydrator for treating petroleum crude ...
The heating pattern of the microwave dehydrator for treating petroleum crude ...
 
Throughput analysis of energy aware routing protocol
Throughput analysis of energy aware routing protocolThroughput analysis of energy aware routing protocol
Throughput analysis of energy aware routing protocol
 
Measuring effort for modifying software package as
Measuring effort for modifying software package asMeasuring effort for modifying software package as
Measuring effort for modifying software package as
 
Control of inverters to support bidirectional power flow in grid connected sy...
Control of inverters to support bidirectional power flow in grid connected sy...Control of inverters to support bidirectional power flow in grid connected sy...
Control of inverters to support bidirectional power flow in grid connected sy...
 
An efficient monitoring system for sports person using wi fi communication
An efficient monitoring system for sports person using wi fi communicationAn efficient monitoring system for sports person using wi fi communication
An efficient monitoring system for sports person using wi fi communication
 
Quality analysis of drinking water in bhopal city
Quality analysis of drinking water in bhopal cityQuality analysis of drinking water in bhopal city
Quality analysis of drinking water in bhopal city
 
Thermodynamic behavior of tetrahydrofuron in p dioxane, methylcyclohexane and...
Thermodynamic behavior of tetrahydrofuron in p dioxane, methylcyclohexane and...Thermodynamic behavior of tetrahydrofuron in p dioxane, methylcyclohexane and...
Thermodynamic behavior of tetrahydrofuron in p dioxane, methylcyclohexane and...
 
Conception of a water level detector (tide gauge) based on a electromagnetic ...
Conception of a water level detector (tide gauge) based on a electromagnetic ...Conception of a water level detector (tide gauge) based on a electromagnetic ...
Conception of a water level detector (tide gauge) based on a electromagnetic ...
 
Prediction of tool wear during turning of en9 work material against coated ca...
Prediction of tool wear during turning of en9 work material against coated ca...Prediction of tool wear during turning of en9 work material against coated ca...
Prediction of tool wear during turning of en9 work material against coated ca...
 
Can fracture mechanics predict damage due disaster of structures
Can fracture mechanics predict damage due disaster of structuresCan fracture mechanics predict damage due disaster of structures
Can fracture mechanics predict damage due disaster of structures
 
Cyclone disaster on housing and coastal area
Cyclone disaster on housing and coastal areaCyclone disaster on housing and coastal area
Cyclone disaster on housing and coastal area
 
Modeling of laminar flow tubular reactor using velocity profile
Modeling of laminar flow tubular reactor using velocity profileModeling of laminar flow tubular reactor using velocity profile
Modeling of laminar flow tubular reactor using velocity profile
 

Similar to Experimental study on the behaviour of retempered concrete

Experimental Investigation on Concrete with coarse Aggregate Replaced with Wa...
Experimental Investigation on Concrete with coarse Aggregate Replaced with Wa...Experimental Investigation on Concrete with coarse Aggregate Replaced with Wa...
Experimental Investigation on Concrete with coarse Aggregate Replaced with Wa...IRJET Journal
 
EXPERIMENTAL INVESTIGATION ON CONCRETE USING RECYCLED COARSE AGGREGATE
EXPERIMENTAL INVESTIGATION ON CONCRETE USING RECYCLED COARSE AGGREGATEEXPERIMENTAL INVESTIGATION ON CONCRETE USING RECYCLED COARSE AGGREGATE
EXPERIMENTAL INVESTIGATION ON CONCRETE USING RECYCLED COARSE AGGREGATEIRJET Journal
 
An Investigation on Strength and Durability of Cement Concrete Partially Repl...
An Investigation on Strength and Durability of Cement Concrete Partially Repl...An Investigation on Strength and Durability of Cement Concrete Partially Repl...
An Investigation on Strength and Durability of Cement Concrete Partially Repl...IRJET Journal
 
Study of corrosion of reinforced steel bars in recycled aggregate concrete wi...
Study of corrosion of reinforced steel bars in recycled aggregate concrete wi...Study of corrosion of reinforced steel bars in recycled aggregate concrete wi...
Study of corrosion of reinforced steel bars in recycled aggregate concrete wi...eSAT Journals
 
Study of corrosion of reinforced steel bars in recycled aggregate concrete wi...
Study of corrosion of reinforced steel bars in recycled aggregate concrete wi...Study of corrosion of reinforced steel bars in recycled aggregate concrete wi...
Study of corrosion of reinforced steel bars in recycled aggregate concrete wi...eSAT Publishing House
 
Use of building demolished waste as coarse aggregate
Use of building demolished waste as coarse aggregateUse of building demolished waste as coarse aggregate
Use of building demolished waste as coarse aggregateeSAT Publishing House
 
Study on compressive strength of concrete by using treated domestic waste wat...
Study on compressive strength of concrete by using treated domestic waste wat...Study on compressive strength of concrete by using treated domestic waste wat...
Study on compressive strength of concrete by using treated domestic waste wat...eSAT Journals
 
Effects of coconut fibers on the properties of concrete
Effects of coconut fibers on the properties of concreteEffects of coconut fibers on the properties of concrete
Effects of coconut fibers on the properties of concreteeSAT Journals
 
IRJET-Replacement of Cement by Granite Powder in Paver Blocks
IRJET-Replacement of Cement by Granite Powder in Paver BlocksIRJET-Replacement of Cement by Granite Powder in Paver Blocks
IRJET-Replacement of Cement by Granite Powder in Paver BlocksIRJET Journal
 
A study on the performance of circular footing embedded in geogrid reinforced...
A study on the performance of circular footing embedded in geogrid reinforced...A study on the performance of circular footing embedded in geogrid reinforced...
A study on the performance of circular footing embedded in geogrid reinforced...eSAT Publishing House
 
Potential utilisation of untreatedtreated textile effluent in concrete
Potential utilisation of untreatedtreated textile effluent in concretePotential utilisation of untreatedtreated textile effluent in concrete
Potential utilisation of untreatedtreated textile effluent in concreteeSAT Publishing House
 
IRJET- Effect of Different Curing on Strength of Concrete
IRJET-  	  Effect of Different Curing on Strength of ConcreteIRJET-  	  Effect of Different Curing on Strength of Concrete
IRJET- Effect of Different Curing on Strength of ConcreteIRJET Journal
 
Self compacting concrete for slip form paving
Self compacting concrete for slip form pavingSelf compacting concrete for slip form paving
Self compacting concrete for slip form pavingeSAT Journals
 
Flexural behaviour of rc beams using foundry sand as partial replacement of f...
Flexural behaviour of rc beams using foundry sand as partial replacement of f...Flexural behaviour of rc beams using foundry sand as partial replacement of f...
Flexural behaviour of rc beams using foundry sand as partial replacement of f...eSAT Journals
 
Flexural behaviour of rc beams using foundry sand as partial replacement of f...
Flexural behaviour of rc beams using foundry sand as partial replacement of f...Flexural behaviour of rc beams using foundry sand as partial replacement of f...
Flexural behaviour of rc beams using foundry sand as partial replacement of f...eSAT Journals
 
Experimental Investigation on Performance of Recycled Concrete Aggregate as C...
Experimental Investigation on Performance of Recycled Concrete Aggregate as C...Experimental Investigation on Performance of Recycled Concrete Aggregate as C...
Experimental Investigation on Performance of Recycled Concrete Aggregate as C...IRJET Journal
 
Experimental studies on performance of steel fiber and polymer modified recyc...
Experimental studies on performance of steel fiber and polymer modified recyc...Experimental studies on performance of steel fiber and polymer modified recyc...
Experimental studies on performance of steel fiber and polymer modified recyc...eSAT Journals
 
EXPERIMENTAL INVESTIGATION OF RECYCLED AGGREGATE CONCRETE USING PRE-SOAKED SL...
EXPERIMENTAL INVESTIGATION OF RECYCLED AGGREGATE CONCRETE USING PRE-SOAKED SL...EXPERIMENTAL INVESTIGATION OF RECYCLED AGGREGATE CONCRETE USING PRE-SOAKED SL...
EXPERIMENTAL INVESTIGATION OF RECYCLED AGGREGATE CONCRETE USING PRE-SOAKED SL...IAEME Publication
 
Behaviour of concrete beams reinforced with glass
Behaviour of concrete beams reinforced with glassBehaviour of concrete beams reinforced with glass
Behaviour of concrete beams reinforced with glasseSAT Publishing House
 
Behaviour of concrete beams reinforced with glass fibre reinforced polymer flats
Behaviour of concrete beams reinforced with glass fibre reinforced polymer flatsBehaviour of concrete beams reinforced with glass fibre reinforced polymer flats
Behaviour of concrete beams reinforced with glass fibre reinforced polymer flatseSAT Journals
 

Similar to Experimental study on the behaviour of retempered concrete (20)

Experimental Investigation on Concrete with coarse Aggregate Replaced with Wa...
Experimental Investigation on Concrete with coarse Aggregate Replaced with Wa...Experimental Investigation on Concrete with coarse Aggregate Replaced with Wa...
Experimental Investigation on Concrete with coarse Aggregate Replaced with Wa...
 
EXPERIMENTAL INVESTIGATION ON CONCRETE USING RECYCLED COARSE AGGREGATE
EXPERIMENTAL INVESTIGATION ON CONCRETE USING RECYCLED COARSE AGGREGATEEXPERIMENTAL INVESTIGATION ON CONCRETE USING RECYCLED COARSE AGGREGATE
EXPERIMENTAL INVESTIGATION ON CONCRETE USING RECYCLED COARSE AGGREGATE
 
An Investigation on Strength and Durability of Cement Concrete Partially Repl...
An Investigation on Strength and Durability of Cement Concrete Partially Repl...An Investigation on Strength and Durability of Cement Concrete Partially Repl...
An Investigation on Strength and Durability of Cement Concrete Partially Repl...
 
Study of corrosion of reinforced steel bars in recycled aggregate concrete wi...
Study of corrosion of reinforced steel bars in recycled aggregate concrete wi...Study of corrosion of reinforced steel bars in recycled aggregate concrete wi...
Study of corrosion of reinforced steel bars in recycled aggregate concrete wi...
 
Study of corrosion of reinforced steel bars in recycled aggregate concrete wi...
Study of corrosion of reinforced steel bars in recycled aggregate concrete wi...Study of corrosion of reinforced steel bars in recycled aggregate concrete wi...
Study of corrosion of reinforced steel bars in recycled aggregate concrete wi...
 
Use of building demolished waste as coarse aggregate
Use of building demolished waste as coarse aggregateUse of building demolished waste as coarse aggregate
Use of building demolished waste as coarse aggregate
 
Study on compressive strength of concrete by using treated domestic waste wat...
Study on compressive strength of concrete by using treated domestic waste wat...Study on compressive strength of concrete by using treated domestic waste wat...
Study on compressive strength of concrete by using treated domestic waste wat...
 
Effects of coconut fibers on the properties of concrete
Effects of coconut fibers on the properties of concreteEffects of coconut fibers on the properties of concrete
Effects of coconut fibers on the properties of concrete
 
IRJET-Replacement of Cement by Granite Powder in Paver Blocks
IRJET-Replacement of Cement by Granite Powder in Paver BlocksIRJET-Replacement of Cement by Granite Powder in Paver Blocks
IRJET-Replacement of Cement by Granite Powder in Paver Blocks
 
A study on the performance of circular footing embedded in geogrid reinforced...
A study on the performance of circular footing embedded in geogrid reinforced...A study on the performance of circular footing embedded in geogrid reinforced...
A study on the performance of circular footing embedded in geogrid reinforced...
 
Potential utilisation of untreatedtreated textile effluent in concrete
Potential utilisation of untreatedtreated textile effluent in concretePotential utilisation of untreatedtreated textile effluent in concrete
Potential utilisation of untreatedtreated textile effluent in concrete
 
IRJET- Effect of Different Curing on Strength of Concrete
IRJET-  	  Effect of Different Curing on Strength of ConcreteIRJET-  	  Effect of Different Curing on Strength of Concrete
IRJET- Effect of Different Curing on Strength of Concrete
 
Self compacting concrete for slip form paving
Self compacting concrete for slip form pavingSelf compacting concrete for slip form paving
Self compacting concrete for slip form paving
 
Flexural behaviour of rc beams using foundry sand as partial replacement of f...
Flexural behaviour of rc beams using foundry sand as partial replacement of f...Flexural behaviour of rc beams using foundry sand as partial replacement of f...
Flexural behaviour of rc beams using foundry sand as partial replacement of f...
 
Flexural behaviour of rc beams using foundry sand as partial replacement of f...
Flexural behaviour of rc beams using foundry sand as partial replacement of f...Flexural behaviour of rc beams using foundry sand as partial replacement of f...
Flexural behaviour of rc beams using foundry sand as partial replacement of f...
 
Experimental Investigation on Performance of Recycled Concrete Aggregate as C...
Experimental Investigation on Performance of Recycled Concrete Aggregate as C...Experimental Investigation on Performance of Recycled Concrete Aggregate as C...
Experimental Investigation on Performance of Recycled Concrete Aggregate as C...
 
Experimental studies on performance of steel fiber and polymer modified recyc...
Experimental studies on performance of steel fiber and polymer modified recyc...Experimental studies on performance of steel fiber and polymer modified recyc...
Experimental studies on performance of steel fiber and polymer modified recyc...
 
EXPERIMENTAL INVESTIGATION OF RECYCLED AGGREGATE CONCRETE USING PRE-SOAKED SL...
EXPERIMENTAL INVESTIGATION OF RECYCLED AGGREGATE CONCRETE USING PRE-SOAKED SL...EXPERIMENTAL INVESTIGATION OF RECYCLED AGGREGATE CONCRETE USING PRE-SOAKED SL...
EXPERIMENTAL INVESTIGATION OF RECYCLED AGGREGATE CONCRETE USING PRE-SOAKED SL...
 
Behaviour of concrete beams reinforced with glass
Behaviour of concrete beams reinforced with glassBehaviour of concrete beams reinforced with glass
Behaviour of concrete beams reinforced with glass
 
Behaviour of concrete beams reinforced with glass fibre reinforced polymer flats
Behaviour of concrete beams reinforced with glass fibre reinforced polymer flatsBehaviour of concrete beams reinforced with glass fibre reinforced polymer flats
Behaviour of concrete beams reinforced with glass fibre reinforced polymer flats
 

More from eSAT Publishing House

Likely impacts of hudhud on the environment of visakhapatnam
Likely impacts of hudhud on the environment of visakhapatnamLikely impacts of hudhud on the environment of visakhapatnam
Likely impacts of hudhud on the environment of visakhapatnameSAT Publishing House
 
Impact of flood disaster in a drought prone area – case study of alampur vill...
Impact of flood disaster in a drought prone area – case study of alampur vill...Impact of flood disaster in a drought prone area – case study of alampur vill...
Impact of flood disaster in a drought prone area – case study of alampur vill...eSAT Publishing House
 
Hudhud cyclone – a severe disaster in visakhapatnam
Hudhud cyclone – a severe disaster in visakhapatnamHudhud cyclone – a severe disaster in visakhapatnam
Hudhud cyclone – a severe disaster in visakhapatnameSAT Publishing House
 
Groundwater investigation using geophysical methods a case study of pydibhim...
Groundwater investigation using geophysical methods  a case study of pydibhim...Groundwater investigation using geophysical methods  a case study of pydibhim...
Groundwater investigation using geophysical methods a case study of pydibhim...eSAT Publishing House
 
Flood related disasters concerned to urban flooding in bangalore, india
Flood related disasters concerned to urban flooding in bangalore, indiaFlood related disasters concerned to urban flooding in bangalore, india
Flood related disasters concerned to urban flooding in bangalore, indiaeSAT Publishing House
 
Enhancing post disaster recovery by optimal infrastructure capacity building
Enhancing post disaster recovery by optimal infrastructure capacity buildingEnhancing post disaster recovery by optimal infrastructure capacity building
Enhancing post disaster recovery by optimal infrastructure capacity buildingeSAT Publishing House
 
Effect of lintel and lintel band on the global performance of reinforced conc...
Effect of lintel and lintel band on the global performance of reinforced conc...Effect of lintel and lintel band on the global performance of reinforced conc...
Effect of lintel and lintel band on the global performance of reinforced conc...eSAT Publishing House
 
Wind damage to trees in the gitam university campus at visakhapatnam by cyclo...
Wind damage to trees in the gitam university campus at visakhapatnam by cyclo...Wind damage to trees in the gitam university campus at visakhapatnam by cyclo...
Wind damage to trees in the gitam university campus at visakhapatnam by cyclo...eSAT Publishing House
 
Wind damage to buildings, infrastrucuture and landscape elements along the be...
Wind damage to buildings, infrastrucuture and landscape elements along the be...Wind damage to buildings, infrastrucuture and landscape elements along the be...
Wind damage to buildings, infrastrucuture and landscape elements along the be...eSAT Publishing House
 
Shear strength of rc deep beam panels – a review
Shear strength of rc deep beam panels – a reviewShear strength of rc deep beam panels – a review
Shear strength of rc deep beam panels – a revieweSAT Publishing House
 
Role of voluntary teams of professional engineers in dissater management – ex...
Role of voluntary teams of professional engineers in dissater management – ex...Role of voluntary teams of professional engineers in dissater management – ex...
Role of voluntary teams of professional engineers in dissater management – ex...eSAT Publishing House
 
Risk analysis and environmental hazard management
Risk analysis and environmental hazard managementRisk analysis and environmental hazard management
Risk analysis and environmental hazard managementeSAT Publishing House
 
Review study on performance of seismically tested repaired shear walls
Review study on performance of seismically tested repaired shear wallsReview study on performance of seismically tested repaired shear walls
Review study on performance of seismically tested repaired shear wallseSAT Publishing House
 
Monitoring and assessment of air quality with reference to dust particles (pm...
Monitoring and assessment of air quality with reference to dust particles (pm...Monitoring and assessment of air quality with reference to dust particles (pm...
Monitoring and assessment of air quality with reference to dust particles (pm...eSAT Publishing House
 
Low cost wireless sensor networks and smartphone applications for disaster ma...
Low cost wireless sensor networks and smartphone applications for disaster ma...Low cost wireless sensor networks and smartphone applications for disaster ma...
Low cost wireless sensor networks and smartphone applications for disaster ma...eSAT Publishing House
 
Coastal zones – seismic vulnerability an analysis from east coast of india
Coastal zones – seismic vulnerability an analysis from east coast of indiaCoastal zones – seismic vulnerability an analysis from east coast of india
Coastal zones – seismic vulnerability an analysis from east coast of indiaeSAT Publishing House
 
Assessment of seismic susceptibility of rc buildings
Assessment of seismic susceptibility of rc buildingsAssessment of seismic susceptibility of rc buildings
Assessment of seismic susceptibility of rc buildingseSAT Publishing House
 
A geophysical insight of earthquake occurred on 21 st may 2014 off paradip, b...
A geophysical insight of earthquake occurred on 21 st may 2014 off paradip, b...A geophysical insight of earthquake occurred on 21 st may 2014 off paradip, b...
A geophysical insight of earthquake occurred on 21 st may 2014 off paradip, b...eSAT Publishing House
 
Effect of hudhud cyclone on the development of visakhapatnam as smart and gre...
Effect of hudhud cyclone on the development of visakhapatnam as smart and gre...Effect of hudhud cyclone on the development of visakhapatnam as smart and gre...
Effect of hudhud cyclone on the development of visakhapatnam as smart and gre...eSAT Publishing House
 
Disaster recovery sustainable housing
Disaster recovery sustainable housingDisaster recovery sustainable housing
Disaster recovery sustainable housingeSAT Publishing House
 

More from eSAT Publishing House (20)

Likely impacts of hudhud on the environment of visakhapatnam
Likely impacts of hudhud on the environment of visakhapatnamLikely impacts of hudhud on the environment of visakhapatnam
Likely impacts of hudhud on the environment of visakhapatnam
 
Impact of flood disaster in a drought prone area – case study of alampur vill...
Impact of flood disaster in a drought prone area – case study of alampur vill...Impact of flood disaster in a drought prone area – case study of alampur vill...
Impact of flood disaster in a drought prone area – case study of alampur vill...
 
Hudhud cyclone – a severe disaster in visakhapatnam
Hudhud cyclone – a severe disaster in visakhapatnamHudhud cyclone – a severe disaster in visakhapatnam
Hudhud cyclone – a severe disaster in visakhapatnam
 
Groundwater investigation using geophysical methods a case study of pydibhim...
Groundwater investigation using geophysical methods  a case study of pydibhim...Groundwater investigation using geophysical methods  a case study of pydibhim...
Groundwater investigation using geophysical methods a case study of pydibhim...
 
Flood related disasters concerned to urban flooding in bangalore, india
Flood related disasters concerned to urban flooding in bangalore, indiaFlood related disasters concerned to urban flooding in bangalore, india
Flood related disasters concerned to urban flooding in bangalore, india
 
Enhancing post disaster recovery by optimal infrastructure capacity building
Enhancing post disaster recovery by optimal infrastructure capacity buildingEnhancing post disaster recovery by optimal infrastructure capacity building
Enhancing post disaster recovery by optimal infrastructure capacity building
 
Effect of lintel and lintel band on the global performance of reinforced conc...
Effect of lintel and lintel band on the global performance of reinforced conc...Effect of lintel and lintel band on the global performance of reinforced conc...
Effect of lintel and lintel band on the global performance of reinforced conc...
 
Wind damage to trees in the gitam university campus at visakhapatnam by cyclo...
Wind damage to trees in the gitam university campus at visakhapatnam by cyclo...Wind damage to trees in the gitam university campus at visakhapatnam by cyclo...
Wind damage to trees in the gitam university campus at visakhapatnam by cyclo...
 
Wind damage to buildings, infrastrucuture and landscape elements along the be...
Wind damage to buildings, infrastrucuture and landscape elements along the be...Wind damage to buildings, infrastrucuture and landscape elements along the be...
Wind damage to buildings, infrastrucuture and landscape elements along the be...
 
Shear strength of rc deep beam panels – a review
Shear strength of rc deep beam panels – a reviewShear strength of rc deep beam panels – a review
Shear strength of rc deep beam panels – a review
 
Role of voluntary teams of professional engineers in dissater management – ex...
Role of voluntary teams of professional engineers in dissater management – ex...Role of voluntary teams of professional engineers in dissater management – ex...
Role of voluntary teams of professional engineers in dissater management – ex...
 
Risk analysis and environmental hazard management
Risk analysis and environmental hazard managementRisk analysis and environmental hazard management
Risk analysis and environmental hazard management
 
Review study on performance of seismically tested repaired shear walls
Review study on performance of seismically tested repaired shear wallsReview study on performance of seismically tested repaired shear walls
Review study on performance of seismically tested repaired shear walls
 
Monitoring and assessment of air quality with reference to dust particles (pm...
Monitoring and assessment of air quality with reference to dust particles (pm...Monitoring and assessment of air quality with reference to dust particles (pm...
Monitoring and assessment of air quality with reference to dust particles (pm...
 
Low cost wireless sensor networks and smartphone applications for disaster ma...
Low cost wireless sensor networks and smartphone applications for disaster ma...Low cost wireless sensor networks and smartphone applications for disaster ma...
Low cost wireless sensor networks and smartphone applications for disaster ma...
 
Coastal zones – seismic vulnerability an analysis from east coast of india
Coastal zones – seismic vulnerability an analysis from east coast of indiaCoastal zones – seismic vulnerability an analysis from east coast of india
Coastal zones – seismic vulnerability an analysis from east coast of india
 
Assessment of seismic susceptibility of rc buildings
Assessment of seismic susceptibility of rc buildingsAssessment of seismic susceptibility of rc buildings
Assessment of seismic susceptibility of rc buildings
 
A geophysical insight of earthquake occurred on 21 st may 2014 off paradip, b...
A geophysical insight of earthquake occurred on 21 st may 2014 off paradip, b...A geophysical insight of earthquake occurred on 21 st may 2014 off paradip, b...
A geophysical insight of earthquake occurred on 21 st may 2014 off paradip, b...
 
Effect of hudhud cyclone on the development of visakhapatnam as smart and gre...
Effect of hudhud cyclone on the development of visakhapatnam as smart and gre...Effect of hudhud cyclone on the development of visakhapatnam as smart and gre...
Effect of hudhud cyclone on the development of visakhapatnam as smart and gre...
 
Disaster recovery sustainable housing
Disaster recovery sustainable housingDisaster recovery sustainable housing
Disaster recovery sustainable housing
 

Recently uploaded

Call Girls Pimpri Chinchwad Call Me 7737669865 Budget Friendly No Advance Boo...
Call Girls Pimpri Chinchwad Call Me 7737669865 Budget Friendly No Advance Boo...Call Girls Pimpri Chinchwad Call Me 7737669865 Budget Friendly No Advance Boo...
Call Girls Pimpri Chinchwad Call Me 7737669865 Budget Friendly No Advance Boo...roncy bisnoi
 
College Call Girls Nashik Nehal 7001305949 Independent Escort Service Nashik
College Call Girls Nashik Nehal 7001305949 Independent Escort Service NashikCollege Call Girls Nashik Nehal 7001305949 Independent Escort Service Nashik
College Call Girls Nashik Nehal 7001305949 Independent Escort Service NashikCall Girls in Nagpur High Profile
 
Sheet Pile Wall Design and Construction: A Practical Guide for Civil Engineer...
Sheet Pile Wall Design and Construction: A Practical Guide for Civil Engineer...Sheet Pile Wall Design and Construction: A Practical Guide for Civil Engineer...
Sheet Pile Wall Design and Construction: A Practical Guide for Civil Engineer...Dr.Costas Sachpazis
 
Online banking management system project.pdf
Online banking management system project.pdfOnline banking management system project.pdf
Online banking management system project.pdfKamal Acharya
 
High Profile Call Girls Nagpur Meera Call 7001035870 Meet With Nagpur Escorts
High Profile Call Girls Nagpur Meera Call 7001035870 Meet With Nagpur EscortsHigh Profile Call Girls Nagpur Meera Call 7001035870 Meet With Nagpur Escorts
High Profile Call Girls Nagpur Meera Call 7001035870 Meet With Nagpur EscortsCall Girls in Nagpur High Profile
 
(ANJALI) Dange Chowk Call Girls Just Call 7001035870 [ Cash on Delivery ] Pun...
(ANJALI) Dange Chowk Call Girls Just Call 7001035870 [ Cash on Delivery ] Pun...(ANJALI) Dange Chowk Call Girls Just Call 7001035870 [ Cash on Delivery ] Pun...
(ANJALI) Dange Chowk Call Girls Just Call 7001035870 [ Cash on Delivery ] Pun...ranjana rawat
 
Extrusion Processes and Their Limitations
Extrusion Processes and Their LimitationsExtrusion Processes and Their Limitations
Extrusion Processes and Their Limitations120cr0395
 
The Most Attractive Pune Call Girls Manchar 8250192130 Will You Miss This Cha...
The Most Attractive Pune Call Girls Manchar 8250192130 Will You Miss This Cha...The Most Attractive Pune Call Girls Manchar 8250192130 Will You Miss This Cha...
The Most Attractive Pune Call Girls Manchar 8250192130 Will You Miss This Cha...ranjana rawat
 
Structural Analysis and Design of Foundations: A Comprehensive Handbook for S...
Structural Analysis and Design of Foundations: A Comprehensive Handbook for S...Structural Analysis and Design of Foundations: A Comprehensive Handbook for S...
Structural Analysis and Design of Foundations: A Comprehensive Handbook for S...Dr.Costas Sachpazis
 
(ANVI) Koregaon Park Call Girls Just Call 7001035870 [ Cash on Delivery ] Pun...
(ANVI) Koregaon Park Call Girls Just Call 7001035870 [ Cash on Delivery ] Pun...(ANVI) Koregaon Park Call Girls Just Call 7001035870 [ Cash on Delivery ] Pun...
(ANVI) Koregaon Park Call Girls Just Call 7001035870 [ Cash on Delivery ] Pun...ranjana rawat
 
Top Rated Pune Call Girls Budhwar Peth ⟟ 6297143586 ⟟ Call Me For Genuine Se...
Top Rated  Pune Call Girls Budhwar Peth ⟟ 6297143586 ⟟ Call Me For Genuine Se...Top Rated  Pune Call Girls Budhwar Peth ⟟ 6297143586 ⟟ Call Me For Genuine Se...
Top Rated Pune Call Girls Budhwar Peth ⟟ 6297143586 ⟟ Call Me For Genuine Se...Call Girls in Nagpur High Profile
 
Introduction and different types of Ethernet.pptx
Introduction and different types of Ethernet.pptxIntroduction and different types of Ethernet.pptx
Introduction and different types of Ethernet.pptxupamatechverse
 
Introduction to Multiple Access Protocol.pptx
Introduction to Multiple Access Protocol.pptxIntroduction to Multiple Access Protocol.pptx
Introduction to Multiple Access Protocol.pptxupamatechverse
 
Introduction to IEEE STANDARDS and its different types.pptx
Introduction to IEEE STANDARDS and its different types.pptxIntroduction to IEEE STANDARDS and its different types.pptx
Introduction to IEEE STANDARDS and its different types.pptxupamatechverse
 
High Profile Call Girls Nagpur Isha Call 7001035870 Meet With Nagpur Escorts
High Profile Call Girls Nagpur Isha Call 7001035870 Meet With Nagpur EscortsHigh Profile Call Girls Nagpur Isha Call 7001035870 Meet With Nagpur Escorts
High Profile Call Girls Nagpur Isha Call 7001035870 Meet With Nagpur Escortsranjana rawat
 
Russian Call Girls in Nagpur Grishma Call 7001035870 Meet With Nagpur Escorts
Russian Call Girls in Nagpur Grishma Call 7001035870 Meet With Nagpur EscortsRussian Call Girls in Nagpur Grishma Call 7001035870 Meet With Nagpur Escorts
Russian Call Girls in Nagpur Grishma Call 7001035870 Meet With Nagpur EscortsCall Girls in Nagpur High Profile
 
Call for Papers - Educational Administration: Theory and Practice, E-ISSN: 21...
Call for Papers - Educational Administration: Theory and Practice, E-ISSN: 21...Call for Papers - Educational Administration: Theory and Practice, E-ISSN: 21...
Call for Papers - Educational Administration: Theory and Practice, E-ISSN: 21...Christo Ananth
 
MANUFACTURING PROCESS-II UNIT-1 THEORY OF METAL CUTTING
MANUFACTURING PROCESS-II UNIT-1 THEORY OF METAL CUTTINGMANUFACTURING PROCESS-II UNIT-1 THEORY OF METAL CUTTING
MANUFACTURING PROCESS-II UNIT-1 THEORY OF METAL CUTTINGSIVASHANKAR N
 

Recently uploaded (20)

Call Girls Pimpri Chinchwad Call Me 7737669865 Budget Friendly No Advance Boo...
Call Girls Pimpri Chinchwad Call Me 7737669865 Budget Friendly No Advance Boo...Call Girls Pimpri Chinchwad Call Me 7737669865 Budget Friendly No Advance Boo...
Call Girls Pimpri Chinchwad Call Me 7737669865 Budget Friendly No Advance Boo...
 
College Call Girls Nashik Nehal 7001305949 Independent Escort Service Nashik
College Call Girls Nashik Nehal 7001305949 Independent Escort Service NashikCollege Call Girls Nashik Nehal 7001305949 Independent Escort Service Nashik
College Call Girls Nashik Nehal 7001305949 Independent Escort Service Nashik
 
Sheet Pile Wall Design and Construction: A Practical Guide for Civil Engineer...
Sheet Pile Wall Design and Construction: A Practical Guide for Civil Engineer...Sheet Pile Wall Design and Construction: A Practical Guide for Civil Engineer...
Sheet Pile Wall Design and Construction: A Practical Guide for Civil Engineer...
 
Online banking management system project.pdf
Online banking management system project.pdfOnline banking management system project.pdf
Online banking management system project.pdf
 
High Profile Call Girls Nagpur Meera Call 7001035870 Meet With Nagpur Escorts
High Profile Call Girls Nagpur Meera Call 7001035870 Meet With Nagpur EscortsHigh Profile Call Girls Nagpur Meera Call 7001035870 Meet With Nagpur Escorts
High Profile Call Girls Nagpur Meera Call 7001035870 Meet With Nagpur Escorts
 
(ANJALI) Dange Chowk Call Girls Just Call 7001035870 [ Cash on Delivery ] Pun...
(ANJALI) Dange Chowk Call Girls Just Call 7001035870 [ Cash on Delivery ] Pun...(ANJALI) Dange Chowk Call Girls Just Call 7001035870 [ Cash on Delivery ] Pun...
(ANJALI) Dange Chowk Call Girls Just Call 7001035870 [ Cash on Delivery ] Pun...
 
Extrusion Processes and Their Limitations
Extrusion Processes and Their LimitationsExtrusion Processes and Their Limitations
Extrusion Processes and Their Limitations
 
The Most Attractive Pune Call Girls Manchar 8250192130 Will You Miss This Cha...
The Most Attractive Pune Call Girls Manchar 8250192130 Will You Miss This Cha...The Most Attractive Pune Call Girls Manchar 8250192130 Will You Miss This Cha...
The Most Attractive Pune Call Girls Manchar 8250192130 Will You Miss This Cha...
 
Structural Analysis and Design of Foundations: A Comprehensive Handbook for S...
Structural Analysis and Design of Foundations: A Comprehensive Handbook for S...Structural Analysis and Design of Foundations: A Comprehensive Handbook for S...
Structural Analysis and Design of Foundations: A Comprehensive Handbook for S...
 
(ANVI) Koregaon Park Call Girls Just Call 7001035870 [ Cash on Delivery ] Pun...
(ANVI) Koregaon Park Call Girls Just Call 7001035870 [ Cash on Delivery ] Pun...(ANVI) Koregaon Park Call Girls Just Call 7001035870 [ Cash on Delivery ] Pun...
(ANVI) Koregaon Park Call Girls Just Call 7001035870 [ Cash on Delivery ] Pun...
 
Roadmap to Membership of RICS - Pathways and Routes
Roadmap to Membership of RICS - Pathways and RoutesRoadmap to Membership of RICS - Pathways and Routes
Roadmap to Membership of RICS - Pathways and Routes
 
Top Rated Pune Call Girls Budhwar Peth ⟟ 6297143586 ⟟ Call Me For Genuine Se...
Top Rated  Pune Call Girls Budhwar Peth ⟟ 6297143586 ⟟ Call Me For Genuine Se...Top Rated  Pune Call Girls Budhwar Peth ⟟ 6297143586 ⟟ Call Me For Genuine Se...
Top Rated Pune Call Girls Budhwar Peth ⟟ 6297143586 ⟟ Call Me For Genuine Se...
 
Introduction and different types of Ethernet.pptx
Introduction and different types of Ethernet.pptxIntroduction and different types of Ethernet.pptx
Introduction and different types of Ethernet.pptx
 
(INDIRA) Call Girl Aurangabad Call Now 8617697112 Aurangabad Escorts 24x7
(INDIRA) Call Girl Aurangabad Call Now 8617697112 Aurangabad Escorts 24x7(INDIRA) Call Girl Aurangabad Call Now 8617697112 Aurangabad Escorts 24x7
(INDIRA) Call Girl Aurangabad Call Now 8617697112 Aurangabad Escorts 24x7
 
Introduction to Multiple Access Protocol.pptx
Introduction to Multiple Access Protocol.pptxIntroduction to Multiple Access Protocol.pptx
Introduction to Multiple Access Protocol.pptx
 
Introduction to IEEE STANDARDS and its different types.pptx
Introduction to IEEE STANDARDS and its different types.pptxIntroduction to IEEE STANDARDS and its different types.pptx
Introduction to IEEE STANDARDS and its different types.pptx
 
High Profile Call Girls Nagpur Isha Call 7001035870 Meet With Nagpur Escorts
High Profile Call Girls Nagpur Isha Call 7001035870 Meet With Nagpur EscortsHigh Profile Call Girls Nagpur Isha Call 7001035870 Meet With Nagpur Escorts
High Profile Call Girls Nagpur Isha Call 7001035870 Meet With Nagpur Escorts
 
Russian Call Girls in Nagpur Grishma Call 7001035870 Meet With Nagpur Escorts
Russian Call Girls in Nagpur Grishma Call 7001035870 Meet With Nagpur EscortsRussian Call Girls in Nagpur Grishma Call 7001035870 Meet With Nagpur Escorts
Russian Call Girls in Nagpur Grishma Call 7001035870 Meet With Nagpur Escorts
 
Call for Papers - Educational Administration: Theory and Practice, E-ISSN: 21...
Call for Papers - Educational Administration: Theory and Practice, E-ISSN: 21...Call for Papers - Educational Administration: Theory and Practice, E-ISSN: 21...
Call for Papers - Educational Administration: Theory and Practice, E-ISSN: 21...
 
MANUFACTURING PROCESS-II UNIT-1 THEORY OF METAL CUTTING
MANUFACTURING PROCESS-II UNIT-1 THEORY OF METAL CUTTINGMANUFACTURING PROCESS-II UNIT-1 THEORY OF METAL CUTTING
MANUFACTURING PROCESS-II UNIT-1 THEORY OF METAL CUTTING
 

Experimental study on the behaviour of retempered concrete

  • 1. IJRET: International Journal of Research in Engineering and Technology eISSN: 2319-1163 | pISSN: 2321-7308 _______________________________________________________________________________________ Volume: 03 Special Issue: 11 | NCAMESHE - 2014 | Jun-2014, Available @ http://www.ijret.org 256 EXPERIMENTAL STUDY ON THE BEHAVIOUR OF RETEMPERED CONCRETE K. Uma Shankar1, K. Arun Prakash2, M. Harshavardana Balaji3, S. Pradep Kumar4 1Assistant Professor, Department of Civil Engineering, Knowledge Institute of Technology, Kakkapalayam, Salem – 637 504, Tamil Nadu, India 2Assistant Professor, Department of Civil Engineering, Knowledge Institute of Technology, Kakkapalayam, Salem – 637 504, Tamil Nadu, India 3Assistant Professor, Department of Civil Engineering, Knowledge Institute of Technology, Kakkapalayam, Salem – 637 504, Tamil Nadu, India 4Assistant Professor, Department of Civil Engineering, Knowledge Institute of Technology, Kakkapalayam, Salem – 637 504, Tamil Nadu, India Abstract Ready–mixed concrete industries, are faced with a common problem known as casting delay, which usually results in a considerable loss of workability, so that concrete may be unworkable. On the other hand, improper methods of handling, lack of site organization, work scheduling and breakdown of equipment are some other causes of unexpected long delays. In such situations engineers at site, many a time reject the concrete partially set and unduly stiffened due to the time elapsed between mixing and placing. It is required to see whether such a stiffened concrete could be used on work without undue harm with use of admixtures. The process of remixing of concrete, if necessary, with addition of just the required quantity of water is known as “retempering” of concrete. The main objective of this research work is to study the behaviour and quality of retempered concrete and making it acceptable in concrete industry which would otherwise go as waste, thus saving the man hours, money and material. To achieve the above objective the workability, near surface characteristics and strength properties of retempered concrete at different time intervals such as, after 15 min, 30 min, 45 min, 60 min, 75 min, 90 min, 105 min and 120 min are found. Keywords: Retempering, workability, near surface characteristics, strength, behaviour, slump. ---------------------------------------------------------------------***-------------------------------------------------------------------- 1. INTRODUCTION Concrete industries and, especially, ready-mixed concrete industries, are faced with a common problem known as casting delay, which usually results in a considerable loss of workability, so that concrete may be unworkable. Delay in the production and delivery of ready-mixed concrete is inevitable, which is influenced by the location of construction sites in relation to the central batching plant and traffic conditions on the route. On the other hand, improper methods of handling, lack of site organization, work scheduling and breakdown of equipment are some other causes of unexpected long delays. The practice of retempering is frequently performed to restore the initial slump and keep concrete workable at construction sites in order to cope with the need for expediting casting operations and reducing consolidation efforts. Retempering of concrete with water, superplasticizers or a combination of both, are the most common variants for resolving slump loss of concrete. However it is well-known that retempering with water alone results in a substantial strength loss, since extra water increases the water to cement ratio of the concrete mixture. In the case of ready-mixed concrete, when concrete is observed at the delivery point to have a lower-than- specified workability, there may be one or more of three possible reasons: (a) Insufficient water batched initially (b) a higher rate of evaporation (or)(absorption by aggregate) than anticipated and (c) a higher rate of hydration than expected. Based on established research, the retempering water added to offset reduction in workability, due to reasons (a) or (b), will not result in strength reduction, whereas extra water to combat (c) will result in a lower strength, due to some increase in the water to cement ratio. On the other hand, retempering with a superplasticizer would be beneficial in terms of the strength loss experienced [1]. One of the adverse effects of hot weather concreting is loss of slump. Delay in the delivery of ready mixed concrete has the same result and leads many people in the concrete industry to regain the original slump by adding water, a process known as 'retempering'. Ready-mixed (RMC) concrete, which is mixed at the plant, using a normal, well- designed concrete mix, should arrive at its destination with sufficient workability to enable it to be properly placed and fully compacted. In such circumstances, where there is a significant period of time between mixing and placing the concrete, there will be a noticeable reduction in the workability of the fresh concrete. If for any reason, the placement of the concrete is unduly delayed, then it may stiffen to an unacceptable degree and site staff would normally insist on the rejection of a batch or otherwise good concrete on the grounds of insufficient workability. If not rejected, excessive vibration would be needed to attempt to fully compact the concrete, with the risk of incomplete
  • 2. IJRET: International Journal of Research in Engineering and Technology eISSN: 2319-1163 | pISSN: 2321-7308 _______________________________________________________________________________________ Volume: 03 Special Issue: 11 | NCAMESHE - 2014 | Jun-2014, Available @ http://www.ijret.org 257 compaction, expensive repair, or, at worst, removal of the hardened concrete. If abnormal slump loss in anticipated or if transport times are significant, then the intelligent use of admixtures can alleviate the potential workability difficulties, although at additional cost, and this practice is common place. However, in cases where unforeseen delay or some other cause has lead unexpectedly to poor workability, retempering of the concrete by water, while normally considered to be bad practice, may, in reality, be contemplated as a possible course of action. The increase in the water content of the concrete immediately prior to discharge will improve the consistency, but it is widely held that there must be a subsequent increase in the water / cement (w/c) ratio which will be detrimental to the hardened concrete. Adding water to a plastic mix to increase slump is an extremely common practice, even though it is not recommended because it increases the porosity of concrete. Concrete often arrives on site more than half an hour after initial mixing. Placement operations can take anywhere from 10 to 60 minutes, depending on the field conditions and the size of the load. When the slump decreases to an unacceptable level during the operations, water is added to the mix and, very often, experienced field inspectors will tolerate what can be termed 'reasonable' retempering, i.e., enough to increase slump by 50 or 60 mm [2]. 2. MATERIALS AND METHODOLOGY In this experimental work, ordinary Portland cement (OPC) 43 grade with cement content of 413.33 Kg /m3 conforming to IS: 8112 – 1989 [3] was used. Low calcium, class F dry fly ash from the silos of Raichur thermal power station conforming to IS: 3812 (Part 1) – 2003 [4] was used. Locally available river sand with specific gravity 2.58 belonging to zone II and locally available crushed angular aggregates of maximum nominal size 20mmwith specific gravity 2.61 were used confirming toIS: 383–1970 [5] and Water fit for drinking was used. 2.1 Methodology In this experimentation, the mix design was done as per IS: 10262 – 2009 [6] and the obtained mix proportion is 1:1.58:2.71 with W/C of 0.45. The quality of retempered concrete was checked w.r.t the following four different cases  Retempered concrete without any addition  Retempered concrete with extra 5% cement + extra 5% water  Retempered concrete with fly ash (20% replacement by cement)  Retempered concrete with fly ash (20% replacement by cement) and extra 5% cement +extra 5% water After thorough mixing of all the ingredients in dry state, the required quantity of water was added in the mix and thoroughly mixed. At this stage, the fresh concrete was kept for 15 minutes retempering time and thereafter workability tests were conducted, such as slump cone test, compaction factor test and Vee-Bee consistometer test. After conducting these tests the fresh concrete was poured into the moulds and the specimens were cast with sufficient compaction through tamping rod and vibrating table. This forms the retempered concrete for 15 minutes. Similarly the specimens were prepared with a retempering time of 30 minutes, 45 minutes, 60 minutes, 75 minutes, 90 minutes, 105 minutes and 120 minutes for all the above four combinations. All the specimens were demoulded after 24 hours of their casting and were transferred to curing tank to cure them for 28 days. After 28 days of curing the specimens were tested for the compressive strength, tensile strength, flexural strength and shear strength as per IS specifications. Near surface characteristic tests such as water absorption test and sorptivity tests were conducted to find percentage water absorption and sorptivity of retempered concrete. The sorptivity test determines the rate of capillary–rise absorption by a concrete cubes which rests on small supports in a manner such that only the lowest 30 mm of the cube is submerged. The increase in the water level of the prism with time is recorded. It has been shown that there exists a relation of the form, S = Where S = sorptivity in mm/min0.5. i = depth of water level increased by capillary action, expressed in mm. t = time measured in minutes at which the depth determined [7]. For compressive strength test, the cubes of size 150 x 150 x 150 mm were cast and tested under compression testing machine of 2000 kN capacity as per IS: 516-1959 [8]. For splitting tensile strength test, the cylinders of 150 mm diameter and length 300 mm were cast and were tested under compression testing machine as per IS: 5816-1999 [9]. For flexural strength test, beams of dimension 100 x 100 x 500 mm were cast and were tested on an effective span of 400 mm with two point loading as per IS: 516-1959 [8]. For shear strength test L shaped specimens as shown in fig. 1 were used.
  • 3. IJRET: International Journal of Research in Engineering and Technology eISSN: 2319-1163 | pISSN: 2321-7308 _______________________________________________________________________________________ Volume: 03 Special Issue: 11 | NCAMESHE - 2014 | Jun-2014, Available @ http://www.ijret.org 258 Fig.1 Shear test on L shaped specimen The specimen was centrally placed on the compression testing machine and load is applied continuously and uniformly. The load is increased until the specimen fails and record the maximum load carried by each specimen during the test. Computation of the shear strength was done as follows. Failure load = Shear strength = × 1000 Where, P = Load in kN A = Area of shear surface = 60 x 150 mm2 L1 = 25 mm L2 = 25 mm. 3.0 RESULTS AND DISCUSSIONS Table 1 gives the slump test results of different retempered concrete combinations for different retempering times, and fig. 2 shows the variation of slump. Table 2 gives the compaction factor test results of different retempered concrete combinations for different retempering times, and fig. 3 shows the variation of compaction factor. Table 3 gives the Vee–Bee test results of different retempered concrete combinations for different retempering times, and fig. 4 shows the variation of Vee–Bee time. Table 1: Slump test results Slump (mm) of retempered concrete Retempering time without any with extra 5% with fly ash (20% with fly ash (20% replacement (minutes) cement + extra 5% replacement by by cement) and extra 5% additions water cement) cement + extra 5% water 0 10 15 20 25 15 10 15 20 25 30 10 15 20 25 45 8 12 15 25 60 8 12 15 20 75 5 10 12 20 90 5 8 10 15 105 4 5 8 10 120 0 3 4 5 Table 2: Compaction factor test results Compaction factor of retempered concrete Retempering time without any with extra 5% with fly ash (20% with fly ash (20% replacement (minutes) cement + extra 5% replacement by by cement) and extra 5% additions water cement) cement + extra 5% water
  • 4. IJRET: International Journal of Research in Engineering and Technology eISSN: 2319-1163 | pISSN: 2321-7308 _______________________________________________________________________________________ Volume: 03 Special Issue: 11 | NCAMESHE - 2014 | Jun-2014, Available @ http://www.ijret.org 259 0 0.865 0.869 0.882 0.896 15 0.862 0.868 0.876 0.893 30 0.860 0.868 0.875 0.885 45 0.858 0.866 0.873 0.880 60 0.857 0.861 0.865 0.871 75 0.851 0.859 0.861 0.865 90 0.847 0.854 0.858 0.863 105 0.845 0.851 0.855 0.858 120 0.844 0.848 0.852 0.853 Table 3: Vee–Bee test results Vee Bee time (sec) of retempered concrete Retempering time (minutes) without any additions with extra 5% with fly ash (20% with fly ash (20% replacement cement + extra 5% replacement by by cement) and extra 5% water cement) cement + extra 5% water 0 5 4 3 2 15 5 4 3 2 30 6 5 3 2 45 6 5 4 2 60 6 5 4 3 75 7 6 4 3 90 8 6 5 3 105 8 7 5 4 120 8 7 5 4 Fig. 2 Variation of slump Fig. 3 Variation of compaction factor
  • 5. IJRET: International Journal of Research in Engineering and Technology eISSN: 2319-1163 | pISSN: 2321-7308 _______________________________________________________________________________________ Volume: 03 Special Issue: 11 | NCAMESHE - 2014 | Jun-2014, Available @ http://www.ijret.org 260 Fig. 4 Variation of Vee–Bee time It is observed that workability as measured from slump, compaction factor and Vee–Bee degree go on decreasing as the retempering time increase. This is true for retempered concrete produced without any additions, produced with extra 5% cement and water, produced with 20% replacement of cement by fly ash, and produced with 20% replacement of cement by fly ash with extra 5% cement and water. This is due to the fact that as the retempering time increases the evaporation of water takes place from the concrete mass and also concrete starts losing its plasticity, thereby reducing workability. Thus it can be concluded that the workability goes on decreasing as the retempering time increase. Also it is observed that workability as measured from slump, compaction factor and Vee–Bee degree is more for the retempered concrete produced with 20% replacement of cement by fly ash and with extra 5% cement and water as compared to other categories. Thisis true for all the retempering times.This is due to the fact that addition of fly ash and extra 5% cement and water will help in keeping the concrete in plastic state for more time thus inducing the flow characteristics.Thus it can be concluded that the workability of retempered concrete produced with 20% replacement of cement by fly ash with extra 5% cement and water is high as compared to other categories of retempered concrete. Table 4 gives the water absorption test results of different retempered concrete combinations for different retempering times, and fig. 5 shows the variation of water absorption. Table 5 gives the sorptivity test results of different retempered concrete combinations for different retempering times, and fig. 6 shows the variation of sorptivity. Table 4: Water absorption test results Water absorption (%) of retempered concrete Retempering time (minutes) without any with extra 5% with fly ash (20% with fly ash (20% replacement cement + extra 5% replacement by by cement) and extra 5% additions water cement) cement + extra 5% water 0 0.800 0.776 0.742 0.735 15 0.853 0.805 0.793 0.746 30 0.860 0.835 0.821 0.770 45 0.928 0.875 0.843 0.790 60 0.937 0.899 0.851 0.849 75 0.955 0.939 0.867 0.864 90 0.985 0.953 0.921 0.901 105 1.002 0.968 0.928 0.923 120 1.058 0.991 0.944 0.942 Table 5: Sorptivity test results Sorptivity (mm/min0.5) of retempered concrete without any with extra 5% with fly ash (20% with fly ash (20% replacement (minutes) cement + extra 5% replacement by by cement) and extra 5% additions water cement) cement + extra 5% water 0 4.52 4.39 4.00 3.87 15 4.65 4.52 4.13 4.00
  • 6. IJRET: International Journal of Research in Engineering and Technology eISSN: 2319-1163 | pISSN: 2321-7308 _______________________________________________________________________________________ Volume: 03 Special Issue: 11 | NCAMESHE - 2014 | Jun-2014, Available @ http://www.ijret.org 261 30 4.78 4.65 4.26 4.13 45 4.78 4.65 4.26 4.13 60 4.91 4.65 4.26 4.13 75 4.91 4.78 4.39 4.26 90 5.03 4.91 4.52 4.39 105 5.29 5.03 4.78 4.52 120 5.42 5.16 4.91 4.65 Fig. 5 Variation of water absorption Fig. 6 Variation of sorptivity It is observed that near surface characteristics as measured from water absorption and sorptivity go on increasing as the retempering time increase. This is true for retempered concrete produced without any additions, produced with extra 5% cement and water, produced with 20% replacement of cement by fly ash, and produced with 20% replacement of cement by fly ash with extra 5% cement and water. This is due to the fact that as the retempering time increases the workability decreases. This results in improper compaction of concrete which may lead to many air– voids in the concrete mass, thereby increasing water absorption and sorptivity.Thus it can be concluded that the near surface characteristics such as water absorption and sorptivity goes on increasing as the retempering time increase. Also it is observed that near surface characteristics as measured from water absorption and sorptivity is least for retempered concrete produced with 20% replacement of cement by fly ash with extra 5% cement and water as compared to other categories. This is true for all the retempering times. This is due to the fact that addition of fly ash with extra 5% cement and water induce plasticity to concrete resulting in more workability. This concrete can be easily compacted thereby reducing the air voids. Thus it can be concluded that the near surface characteristics such as water absorption and sorptivity is least for retempered concrete produced with 20% replacement of cement by fly ash with extra 5% cement and water as compared to other categories of retempered concrete. Table 6 gives the results of compressive strength of retempered concrete for different combinations with different retempering times, and fig. 7 shows the variation of compressive strength. Table 7 gives the results of tensile strength of retempered concrete for different combinations with different retempering times, and fig. 8 shows the variation of tensile strength. Table 8 gives the results of flexural strength of retempered concrete for different combinations with different retempering times, and fig. 9 shows the variation of flexural strength. Table 9 gives the results of shear strength of retempered concrete for different combinations with different retempering times, and fig. 10 shows the variation of shear strength. Table 6: Results of compressive strength Compressive strength (MPa) of retempered concrete Retempering time with extra 5% with fly ash with fly ash (20% without any replacement by cement) and (minutes) cement + extra 5% (20% replacement additions extra 5% cement + extra 5% water by cement)
  • 7. IJRET: International Journal of Research in Engineering and Technology eISSN: 2319-1163 | pISSN: 2321-7308 _______________________________________________________________________________________ Volume: 03 Special Issue: 11 | NCAMESHE - 2014 | Jun-2014, Available @ http://www.ijret.org 262 water 0 42.22 42.37 42.67 43.11 15 42.81 43.26 43.41 43.56 30 43.11 43.70 43.85 44.15 45 43.41 44.15 44.44 44.89 60 42.37 42.96 43.11 43.41 75 41.48 42.07 42.37 42.67 90 40.74 41.33 41.63 41.78 105 40.00 40.15 40.44 40.74 120 39.11 39.26 39.56 40.30 Table 7: Results of tensile strength Tensile strength (MPa) of retempered concrete Retempering time with extra 5% with fly ash with fly ash (20% without any replacement by cement) (minutes) cement + extra (20% replacement additions and extra 5% cement + 5% water by cement) extra 5% water 0 3.68 3.77 3.82 3.91 15 3.77 3.87 3.96 4.10 30 3.87 3.96 4.10 4.20 45 3.96 4.15 4.29 4.39 60 3.87 4.01 4.10 4.20 75 3.68 3.87 3.91 3.96 90 3.58 3.68 3.72 3.82 105 3.44 3.49 3.54 3.63 120 3.30 3.39 3.44 3.54 Table 8: Results of flexural strength Flexural strength (MPa) of retempered concrete Retempering time with extra 5% with fly ash with fly ash (20% without any replacement by cement) (minutes) cement + extra (20% replacement additions and extra 5% cement + 5% water by cement) extra 5% water 0 6.47 6.80 7.13 7.40 15 6.93 7.20 7.40 7.67 30 7.20 7.47 7.93 8.07 45 7.73 7.87 8.27 8.73 60 6.80 7.20 7.47 7.87 75 6.47 6.80 7.20 7.60 90 6.07 6.47 6.80 7.33 105 5.67 6.13 6.53 6.80 120 5.47 5.80 6.33 6.60
  • 8. IJRET: International Journal of Research in Engineering and Technology eISSN: 2319-1163 | pISSN: 2321-7308 _______________________________________________________________________________________ Volume: 03 Special Issue: 11 | NCAMESHE - 2014 | Jun-2014, Available @ http://www.ijret.org 263 Table 9: Results of shear strength Shear strength (MPa) of retempered concrete Retempering time with extra 5% with fly ash with fly ash (20% without any replacement by cement) (minutes) cement + extra (20% replacement additions and extra 5% cement + 5% water by cement) extra 5% water 0 3.70 4.07 4.26 4.44 15 4.07 4.26 4.44 4.63 30 4.26 4.63 4.81 5.00 45 4.63 4.81 5.19 5.37 60 4.44 4.63 4.81 5.00 75 3.89 4.07 4.44 4.81 90 3.52 3.70 4.07 4.44 105 3.15 3.33 3.70 4.07 120 2.96 3.15 3.33 3.70 Fig. 7 Variation of compressive strength Fig. 9 Variation of flexural strength Fig. 8 Variation of tensile strength Fig. 10 Variation of shear strength
  • 9. IJRET: International Journal of Research in Engineering and Technology eISSN: 2319-1163 | pISSN: 2321-7308 _______________________________________________________________________________________ Volume: 03 Special Issue: 11 | NCAMESHE - 2014 | Jun-2014, Available @ http://www.ijret.org 264 It is observed that compressive strength, tensile strength, flexural strength and shear strength of retempered concrete goes on increasing up to 45 minutes of retempering time. Thereafter all the strengths start decreasing. This is true for retempered concrete produced without any additions, produced with extra 5% cement and water, produced with 20% replacement of cement by fly ash, and produced with 20% replacement of cement by fly ash with extra 5% cement and water. This is due to the fact that above 45 minutes of retempering time the concrete looses the plasticity seriously and remixing the concrete beyond 45 minutes will not reunite the concrete particles to adhere together. Thus it can be concluded that compressive strength, tensile strength, flexural strength and shear strength of retempered concrete goes on increasing up to 45 minutes of retempering time. Therefore retempering can be allowed up to 45 minutes. Also it is observed that compressive strength, tensile strength, flexural strength and shear strength of concrete is more for retempered concrete produced with 20% replacement of cement by fly ash with extra 5% cement and water as compared to other categories. This is true for all the retempering times. This is due to the fact that addition of fly ash and extra 5% cement and water will help in keeping the concrete in plastic state which helps in thorough compaction of concrete resulting in higher strength.Thus it can be concluded that compressive strength, tensile strength, flexural strength and shear strength of concrete is more for retempered concrete produced with 20% replacement of cement by fly ash with extra 5% cement and water as compared to other categories. 4. CONCLUSIONS Following conclusions can be drawn based on the experimentations conducted on the retempered concrete.  Workability goes on decreasing as the retempering time increase.  Workability of retempered concrete produced with 20% replacement of cement by fly ash with extra 5% cement and water is high as compared to other categories of retempered concrete.  Near surface characteristics such as water absorption and sorptivity goes on increasing as the retempering time increase.  Near surface characteristics such as water absorption and sorptivity is least for retemperedconcrete produced with 20% replacement of cement by fly ash with extra 5% cement and water as compared to other categories of retempered concrete.  Compressive strength, tensile strength, flexural strength and shear strength of retemperedconcrete goes on increasing up to 45 minutes of retempering time. Therefore retempering can be allowed up to the time of 45 minutes.  Compressive strength, tensile strength, flexural strength and shear strength of concrete is more for retempered concrete produced with 20% replacement of cement by fly ash with extra 5% cement and water as compared to other categories. REFERENCES [1]. IS: 8112 – 1989, ―43 Grade ordinary Portland cement—Specifications‖ (First revision),BIS, New Delhi, May 1990. [2]. IS: 3812 (Part 1) – 2003, ―Pulverized fuel ash – Specification‖ (Second revision),BIS, New Delhi, October 2003. [3]. IS: 383 – 1970, ―Specifications for coarse and fine aggregate from natural sources for concrete‖ (Second revision), BIS, New Delhi, April 1971. [4]. IS: 10262 – 2009, ―Concrete mix proportioning – Guidelines‖ (First revision), BIS, New Delhi, July 2009. [5]. IS: 10262-1982 Recommended Guidelines for Concrete Mix Design. [6]. SANTHAKUMAR.A.R,―Concrete Technology‖, Oxford Publishing & Co., New Delhi, 2007, First Edition. BIOGRAPHIES Prof.K.UmaShankar presently working as Assistant Professor in the department of Civil Engineering at Knowledge Institute of Technology. He has more than 4 years of teaching experience. He has published 5 papers in the reputed International and National journals & Conferences. Mr.K.ArunPrakash is presently working as Assistant Professor in the Department of Civil Engineering at Knowledge Institute of Technology. He has more than 3 years of teaching experience. He has published 1 paper in the International Conference and 2 papers in the National Conferences. Mr.M.Harshavardana Balaji is presently working as Assistant Professor in the Department of Civil Engineering at Knowledge Institute of Technology. He has more than 2 years of teaching experience. He has published 1 paper in the International Conference and 2 papers in the National Conferences. S.PradeepKumar is presently working as Assistant Professor in the Department of Civil Engineering at Knowledge Institute of Technology. He has more than 2 years of teaching experience. He has published 1 paper in the International Conference and 2 papers in the National Conferences.