1. Abstract
2. Introduction
3. Objective
4. Introduction To En-8 Steel
5. Properties Of En-8 Steel
6. Heat Treatment Process
7. Universal Testing Machine
8. Sample Preparation
9. Optical Microscope
10.Comparison Of Microstructures
11.Inference
12.Reference
Steels are generally heat treated in order to achieve desired changes in
their microstructure and mechanical properties. The effect of heat
treatment cycle on the microstructure and some mechanical properties of
EN8 steel have been studied and presented in this presentation. The
heat treatment cycles given are Annealing, normalizing, hardening and
tempering are the most important heat treatments often used to modify
the microstructure and mechanical properties of engineering materials
particularly steels.
Sample of steel is purchased and various specimens are prepared for
tests of mechanical properties, the changes in properties are examined
and studied. Finally the heat treated sample was examined in the
microscope. In the specimen, grains were differentiated and impurity
particle could be seen clearly. The microstructure of the specimen was
snapped on 100X, 200X, 500X, and 1000X. Then, analysis and
comparison of the microstructure is done.
 Heat treatment and microstructure studies have always been
a wide area of research for mechanical engineers
 We come across steel in our life on an everyday basis. We
can find its influence in our life in almost everything we do,
we use or we look at. The steel used for this research
however is a medium carbon EN-8 steel AISI 1040. It is
alloyed and it is used to make things like shafts, keys,
stressed pins. The steel with its immense practical
applications are an important component in everybody's life.
 EN8 is a very popular grade of through-hardening medium
carbon steel, which is readily machined able in any
condition. EN8 is suitable for the manufacture of parts such
as general-purpose axles and shafts, gears, bolts and studs.
 To treat the En 8 steel in quenching annealing and normalizing.
 To treat the En 8 steel in single tempering after quenching annealing
and normalizing .
 To measured tensile strength by universal testing machine (UTM) .
 To compare the hardness of En8 steel after quenching annealing and
normalizing.
 To compare the micro-structure of the specimen after different heat
treatment process.
 EN8 is an alloyed medium carbon steel grade with
reasonable tensile strength. It is normally supplied in the cold drawn or
as rolled condition. Tensile properties can vary but are usually
between 500-800 N/mm². EN8 is widely used for applications which
require better properties than mild steel but does not justify the costs of
an alloy steel. EN8 can be flame or induction hardened to produce a
good surface hardness with moderate wear resistance.
 EN8 carbon steel is a common medium carbon and medium tensile steel, with
improved strength over mild steel, through-hardening medium carbon steel.
 Readily machinable in any condition.
 It can be further surface-hardened by induction processes, producing
components with enhanced wear resistance.
 In its heat treated forms possesses good homogenous metallurgical structures,
giving consistent machining properties
 Suitable for the manufacture of parts such as general-purpose axles and shafts,
gears, bolts and studs.
 Good heat treatment results on sections be achievable.
Max Stress 700-850N/mm^2
Yield stress 465N/mm^2 min
Max Elongation 16% min
Impact KCV 28 Joules min
Hardness 201-255 Brinell
MECHANICAL PROPERTIES
En8 specification chemical composition
carbon 0.36-0.44%
silicon 0.10-0.40%
manganese 0.60-1.00%
Sulphur 0.050Max
phosphorus 0.050Max
The sample was received as a round bar. Later on it was cut to desired
specified measurement as per our requirement. Later the specimens
were undergone through various heat treatment processes.
 Heat treatment is a combination of timed heating and cooling
applied to a particular metal or alloy in the solid state in such
ways as to produce certain microstructure and desired
mechanical properties. The heat treatment of steel was done at
different temperatures of 950OC, 975OC, 1000OC, 1025OC by
using muffle furnace. At each temperature 6 samples were kept to
be heated.
 A furnace is a device used for high-
temperature heating.
 A furnace used for many things, such
as the extraction of metal from ore or
in oil refineries and other chemical
plants.
 The heat energy to fuel a furnace may
be supplied directly by
fuel combustion, by electricity such as
the electric arc furnace, or
through induction heating in induction
furnaces.
 It serves as a reactor to provide heats to
the reaction. The design of the furnaces
varies, however the basic features are
most common among all of them.
Specimen of EN-8 steel rod was first preheated at 15OC per minute to 950OC
in a furnace and then held there for 30 minutes such that the temperature
homogeneity occurs at all section of the specimens for austentization. After
holding for 30 minutes, switch off the furnace and open the furnace door to
allow the samples to cool inside the furnace until red heat is gone. Take out the
samples and air cool to 65OC in air take out the samples which are at the
austenitizing temperature, submerge in oil bath, and water quenched to the
room temperature.
To remove any preexisting anomalies of material properties, the sample were
first subject to a careful annealing cycle: preheating to 950OC, hold for 15
min. slow (stepwise) heating to 950OC; 200-400-600-800-950OC; hold for 15
min at each step. Holding for ½ hrs at 950OC, slow cooling and switch off
furnace. Leave samples inside until cooled to 480OC. brisk cooling open
furnace door, cool to room temperature.
Normalizing process for steels is defined as heating the steel to
austenite phase and cooling it in the air. It is carried out by
heating the steel approximately 500C above the upper critical
temperature followed by cooling in air to room temperature, or at
no greater than 1 bar pressure using nitrogen if the process is
being run in a vacuum furnace. Normalizing temperatures usually
vary from 8100c to 9300C.
Temper the EN8 component immediately after quenching whilst tools are still
hand warm. Re-heat the EN8 component to the tempering temperature then
soak for one hour per 25 millimeter of total thickness (2 hours minimum) Cool
in air. For most applications tempering of EN8 will be between 550-660°C.
Sl.
No.
Heat Treated Sample Force (KN)
1.
Quenching
(Without Tempering) 251
2.
Annealing
(Without Tempering) 152
3.
Normalizing
(Without Tempering) 168
4.
Quenching
(With Tempering) 207
5.
Annealing
(With Tempering) 118
6.
Normalizing
(With Tempering) 165
Heat treated samples were
tested for various mechanical
properties. Average HRC
readings were determined by
taking several readings at
different positions on the
samples, using Rockwell
hardness tester. For tensile
properties, standard tensile
specimens were loaded into
400-KN Universal Testing
Machine hooked up to a data
logger.
A machine used to test specimens for tensile strength,
compressive strength, shear strength and to perform bend test
along other important laboratory tests. The primary use of the
testing machine is to create the stress strain diagram.
Once the diagram is generated, a pencil and straight edge or
computer algorithm can be
used to calculate
yield strength,
Young's Modulus,
tensile strength
or total elongation.
Tool Steel
Material
Sample Mark Rockwell
Hardness
C-HRC
Rockwell
Hardness
B-HRB
Brinell
Hardness
HB
EN-8
Annealing
12 91 187
Annealing with
Tempering
1 82 155
Quenching
42 113 392
Quenching
with Tempering
63 - 685
Normalizing
47 115 446
Normalizing
with Tempering
22 99 234
Hardness of EN-8 Steel was determined using Brinell and Rockwell
Proper preparation of metallographic specimens to determine
microstructure and content requires that a rigid step-by-step process
be followed. In sequence, the steps included cutting, mounting,
course grinding, fine grinding, polishing, etching and microscopic
examination. Specimens must be kept clean and preparation
procedure carefully followed in order to reveal accurate
microstructures.
This operation was performed using a power hacksaw. this process is involve
cutting a small piece of the work piece by a tool consisting of a series of
narrowly spaced teeth, called a saw blade. Sawing is used to separate work
parts into two or more pieces, or to cut off an unwanted section of a part.
Grinding is the most common form of abrasive machining. It is a material cutting
process which engages an abrasive tool whose cutting elements are grains of
abrasive material known as grit. These grits are characterized by sharp cutting
points, high hot hardness, chemical stability and wear resistance. The grits are
held together by a suitable bonding material to give shape of an abrasive tool.
Metal Polishing sometimes known as Finishing or Buffing is the process of
removing scratches and abrasions from a surface, and creating the desired
brightness of finish on that surface. Polishing, like using sand paper, consists of
procedures each of which is less abrasive than the previous. A combination of
polishing buffing wheels and compounds are used with a buffing machine or a
household electric drill (pneumatic tools may also be used but only at relatively
low speeds of 4000 rpm max.)
The specimen was placed on the table under the fume hood with the polished
surface up.
1. The surface was cleaned with alcohol and let dried.
2. A few drops of nital solution (2%) were applied to the specimen surface
covering the entire metallic surface of the specimen using the eye dropper.
3. After 20 to 30 seconds. The etchant was rinsed into the sink with the water and
it is quickly rinsed with alcohol.
4. The sample was dried again.
The sample was examined in the optical microscope. In the specimen, grains were
differentiated and impurity particles could be seen clearly.
Metallurgical microscope was used to view the specimen at various magnifications
and the microstructural aspect of the material was noted.
The microstructure of the specimen was snapped on 100X, 200X, 500X, 1000X
zooming lenses.
The optical microscope, often referred to as light
microscope, is a type of microscope which
uses visible light and a system of lenses to
magnify images of small samples.
The image from an optical microscope can be
captured by normal light-sensitive cameras to
generate a micrograph.
Compound optical microscopes are typically used
to examine a smear, a squash preparation, or a
thinly sectioned slice of some material.
A common use of non-transmitted lighting is to
study the thin structure of metals and minerals,
where the light is reflected from the examined
surface.
It can produce a magnified image of a specimen
up to 1000X and, at high magnifications, are used
to study thin specimens as they have a very
limited depth of field.
The figure depicts microstructure of ‘As received material’ (which is
EN-8 steel prior to heat treatment) at 200X zoom, from our objective
point of view we consider this microstructure as our reference for
further analysis. We can observe from this microstructure the pearlite
and ferrite structure clearly. We can also observe non uniformity of
the grain size and its coarse nature, the ferrite and pearlite
microstructure are also non uniform. The material does not possess
good wear resistance.
The quenched specimens would have their austenites transformed to
martensites. These are fine, needle-like structures which are very strong and
hard, but very brittle. The transformation of austenite to martensite by a
diffusion less shear type transformation in quenching is also responsible for
higher hardness obtained and this property is attributed to the effectiveness of
the interstitial carbon in hindering the dislocation motion. After the hardened
steel tempered the prevalent martensite is an unstable structure and the carbon
atoms diffuse from martensite to form a carbide precipitate and the concurrent
formation of ferrite and cementite.
Fig. Quenching with tempering Fig. Quenching without tempering
If we now observed the microstructure of normalized with tempering steel we can
see the coarse grains are produced. The grain size diameter is increased.
Because of tempering the heating temp is low and cooling rate is low so nuclei
formation will be less. The grain boundary is less than the normalized steel, void
also decreases. It increases the dislocation movement because of this ductility of
the material will also increase.
Fig. Normalizing (200X) Fig. Normalizing with
tempering (200X)
If we observe the microstructure of annealing with that of annealing along with
tempering we can see the fine grains are transformed into coarsened grains due
to which void is decreased. The grain size diameter is increased .Because in
tempering the heating temp.is low and cooling rate is low so nuclei formation will
be less. The grain boundary is less than the annealed steel. As a result of
tempering the martensite gets transformed into tempered martensite and thus as
a result hardness of the sample decreases.
Fig. Annealing (200X) Fig. Annealing With
Tempering (200X)
The following conclusion has been drawn from the experimental result and discussion
is made. The EN8 steel are subjected to different heat treatment sequences:
annealing, normalizing, quenching and tempering at different temperatures at 2000C,
4000C, 6000C, 8000C, 9500C. Heat treated specimens were mechanically tested for
tensile properties, ductility, and hardness.
 After quenching the tensile strength and hardness was increased due the formation
of martensitic structure. The crystal grain size was reduced.
 After annealing it is observed that the hardness is reduced which softens the
specimen, the grain size is refined which in turns improves the machinability of EN8
steel.
 After normalizing it is observed that uniform ferrite plus pearlite microstructure is
established and uniform grain size obtained.
 Tempering the specimen after undergoing above process was found to have many
changes like the ductility and toughness was increased with some loss of strength,
hardness and ultimate tensile strength, it also possess good corrosion resistance.
1. krishisanskriti.org/Publication.html
2. O.P. Khanna, material science & metallurgy (Dhanpat Rai Publications,
11th Reprint-2007).
3. Elements of Metallurgy and Engineering Alloys. Product code-05224G, F.C.
Campbell. www.asminternational.org
4. ASM International 1991, ASM Handbook: Heat Treatment, Vol. 4, American
Society for Metals Park, Ohio
5. ASTM E18. 2008, Standard Test Method for Rockwell Hardness of Metallic
Materials, American Society of Testing and Materials.
6. D. A. Fadare, T. G. Fadara and O. Y. Akanbi (2011) ―Effect of Heat
Treatment on Mechanical.
7. Romesh C Sharma, principles of heat treatment of steels (New Age
International Publishers, New Delhi, 2008)
8. International Journal of Engineering Research and Development ISSN:
2278-067X, Volume 2, Issue 1 (July 2012), PP. 07-13 www.ijerd.com
9. Journal of minerals and materials characterization and engineering, 2012,
11, 859-862, published online September 2012
10.Highpeaksteels.com
11.Metals4u.co.uk
STUDY OF MICRO STRUCTURE OF HEAT TREADTED EN8 STEEL

More Related Content

What's hot

cryogenic treatment of metals
cryogenic treatment of metalscryogenic treatment of metals
cryogenic treatment of metalsDeepak Singh
 
Stainless steel piping
Stainless steel pipingStainless steel piping
Stainless steel pipingAmir Razmi
 
Alloy-Effect of Alloying Elements in Iron and Steel.pdf
Alloy-Effect of Alloying Elements in Iron and Steel.pdfAlloy-Effect of Alloying Elements in Iron and Steel.pdf
Alloy-Effect of Alloying Elements in Iron and Steel.pdfAnnamalai Ram
 
Iron Carbon Phase Diagram
Iron Carbon Phase DiagramIron Carbon Phase Diagram
Iron Carbon Phase DiagramJose Surendran
 
TTT diagram and Heat treatment processes
TTT diagram and Heat treatment processesTTT diagram and Heat treatment processes
TTT diagram and Heat treatment processesSaumy Agarwal
 
Metallurgical difficulties in welding of ferritic martensitic and duplex sta...
Metallurgical difficulties  in welding of ferritic martensitic and duplex sta...Metallurgical difficulties  in welding of ferritic martensitic and duplex sta...
Metallurgical difficulties in welding of ferritic martensitic and duplex sta...Archunan Ponnukhan
 
rolls for rolling mill
rolls for rolling millrolls for rolling mill
rolls for rolling millCameron KL
 
Phase Diagram & Heat Treatment Of Metals
Phase Diagram & Heat Treatment Of MetalsPhase Diagram & Heat Treatment Of Metals
Phase Diagram & Heat Treatment Of MetalsExplosion Cladding
 
Manufacturing & Applications of Stainless Steels
Manufacturing & Applications of Stainless SteelsManufacturing & Applications of Stainless Steels
Manufacturing & Applications of Stainless SteelsVenkataraman Bandaru
 
Heat treatment of steel
Heat treatment of steelHeat treatment of steel
Heat treatment of steelbanty patel
 
Deoxidation and inclusion control
Deoxidation and inclusion controlDeoxidation and inclusion control
Deoxidation and inclusion controlNikhi Lesh
 
Austempering and Martempering in Metallurgy
Austempering and Martempering in Metallurgy Austempering and Martempering in Metallurgy
Austempering and Martempering in Metallurgy Khushal Hudke
 

What's hot (20)

Types of steels in use
Types of steels in useTypes of steels in use
Types of steels in use
 
cryogenic treatment of metals
cryogenic treatment of metalscryogenic treatment of metals
cryogenic treatment of metals
 
Stainless steel piping
Stainless steel pipingStainless steel piping
Stainless steel piping
 
StainlessSteels.pptx
StainlessSteels.pptxStainlessSteels.pptx
StainlessSteels.pptx
 
Alloy-Effect of Alloying Elements in Iron and Steel.pdf
Alloy-Effect of Alloying Elements in Iron and Steel.pdfAlloy-Effect of Alloying Elements in Iron and Steel.pdf
Alloy-Effect of Alloying Elements in Iron and Steel.pdf
 
Iron Carbon Phase Diagram
Iron Carbon Phase DiagramIron Carbon Phase Diagram
Iron Carbon Phase Diagram
 
Heat treatment of stainless steel
Heat treatment of stainless steelHeat treatment of stainless steel
Heat treatment of stainless steel
 
Heat treatment 2
Heat treatment 2Heat treatment 2
Heat treatment 2
 
Alloy steels
Alloy steelsAlloy steels
Alloy steels
 
TTT diagram and Heat treatment processes
TTT diagram and Heat treatment processesTTT diagram and Heat treatment processes
TTT diagram and Heat treatment processes
 
Metallurgical difficulties in welding of ferritic martensitic and duplex sta...
Metallurgical difficulties  in welding of ferritic martensitic and duplex sta...Metallurgical difficulties  in welding of ferritic martensitic and duplex sta...
Metallurgical difficulties in welding of ferritic martensitic and duplex sta...
 
rolls for rolling mill
rolls for rolling millrolls for rolling mill
rolls for rolling mill
 
Phase Diagram & Heat Treatment Of Metals
Phase Diagram & Heat Treatment Of MetalsPhase Diagram & Heat Treatment Of Metals
Phase Diagram & Heat Treatment Of Metals
 
Manufacturing & Applications of Stainless Steels
Manufacturing & Applications of Stainless SteelsManufacturing & Applications of Stainless Steels
Manufacturing & Applications of Stainless Steels
 
Heat treatment of steel
Heat treatment of steelHeat treatment of steel
Heat treatment of steel
 
Ti alloys
Ti alloysTi alloys
Ti alloys
 
Deoxidation and inclusion control
Deoxidation and inclusion controlDeoxidation and inclusion control
Deoxidation and inclusion control
 
Steel making
Steel makingSteel making
Steel making
 
iron carbon phase diagram
iron carbon  phase diagramiron carbon  phase diagram
iron carbon phase diagram
 
Austempering and Martempering in Metallurgy
Austempering and Martempering in Metallurgy Austempering and Martempering in Metallurgy
Austempering and Martempering in Metallurgy
 

Similar to STUDY OF MICRO STRUCTURE OF HEAT TREADTED EN8 STEEL

Comparison of Mechanical Properties of Austempered, Normalized and As-Weld Ca...
Comparison of Mechanical Properties of Austempered, Normalized and As-Weld Ca...Comparison of Mechanical Properties of Austempered, Normalized and As-Weld Ca...
Comparison of Mechanical Properties of Austempered, Normalized and As-Weld Ca...IJAEMSJORNAL
 
Analysis and Improvement of Distortion of Lathe Machine Main Spindle
Analysis and Improvement of Distortion of Lathe Machine Main SpindleAnalysis and Improvement of Distortion of Lathe Machine Main Spindle
Analysis and Improvement of Distortion of Lathe Machine Main SpindleIRJET Journal
 
Effect of Heat Treatment on Corrosion Behavior of Spring Steels
Effect of Heat Treatment on Corrosion Behavior of Spring SteelsEffect of Heat Treatment on Corrosion Behavior of Spring Steels
Effect of Heat Treatment on Corrosion Behavior of Spring SteelsEditor IJCATR
 
Effect of Subzero Treatment on Microstructure and Material Properties of EN...
Effect of Subzero Treatment on Microstructure and Material  Properties of EN...Effect of Subzero Treatment on Microstructure and Material  Properties of EN...
Effect of Subzero Treatment on Microstructure and Material Properties of EN...IJMER
 
Influence of Heat Treatment on Mechanical Properties of Aisi1040 Steel
Influence of Heat Treatment on Mechanical Properties of Aisi1040 SteelInfluence of Heat Treatment on Mechanical Properties of Aisi1040 Steel
Influence of Heat Treatment on Mechanical Properties of Aisi1040 SteelIOSR Journals
 
Study and Analysis on Heat Treatment Process and Microstructure of Low Carbon...
Study and Analysis on Heat Treatment Process and Microstructure of Low Carbon...Study and Analysis on Heat Treatment Process and Microstructure of Low Carbon...
Study and Analysis on Heat Treatment Process and Microstructure of Low Carbon...IJARTES
 
IJERD (www.ijerd.com) International Journal of Engineering Research and Devel...
IJERD (www.ijerd.com) International Journal of Engineering Research and Devel...IJERD (www.ijerd.com) International Journal of Engineering Research and Devel...
IJERD (www.ijerd.com) International Journal of Engineering Research and Devel...IJERD Editor
 
IJERD(www.ijerd.com)International Journal of Engineering Research and Develop...
IJERD(www.ijerd.com)International Journal of Engineering Research and Develop...IJERD(www.ijerd.com)International Journal of Engineering Research and Develop...
IJERD(www.ijerd.com)International Journal of Engineering Research and Develop...IJERD Editor
 
Effect of Subzero Treatment on Microstructure and Material Properties of EN24...
Effect of Subzero Treatment on Microstructure and Material Properties of EN24...Effect of Subzero Treatment on Microstructure and Material Properties of EN24...
Effect of Subzero Treatment on Microstructure and Material Properties of EN24...IJMER
 
Effect of Hardness and Wear Resistance on En 353 Steel by Heat Treatment
Effect of Hardness and Wear Resistance on En 353 Steel by Heat  Treatment Effect of Hardness and Wear Resistance on En 353 Steel by Heat  Treatment
Effect of Hardness and Wear Resistance on En 353 Steel by Heat Treatment IJMER
 
Study on Influence of heat treatment on Tribological properties of mild steel
Study on Influence of heat treatment on Tribological properties of mild steelStudy on Influence of heat treatment on Tribological properties of mild steel
Study on Influence of heat treatment on Tribological properties of mild steeldbpublications
 
Development of laboratory scale salt bath furnace
Development of laboratory scale salt bath furnaceDevelopment of laboratory scale salt bath furnace
Development of laboratory scale salt bath furnaceAlexander Decker
 
Mechanical property assessment of austempered and conventionally hardened aisi
Mechanical property assessment of austempered and conventionally hardened aisiMechanical property assessment of austempered and conventionally hardened aisi
Mechanical property assessment of austempered and conventionally hardened aisiIAEME Publication
 
An assessment of the microstraft
An assessment of the microstraftAn assessment of the microstraft
An assessment of the microstraftAlexander Decker
 
New ppt cold working process
New ppt cold working processNew ppt cold working process
New ppt cold working processShikhar Saraswat
 
Steady state thermal analysis of a 4-stroke single
Steady state thermal analysis of a 4-stroke singleSteady state thermal analysis of a 4-stroke single
Steady state thermal analysis of a 4-stroke singleVarun Bhalerao
 
Repairing of kiln shell crack
Repairing of kiln shell crackRepairing of kiln shell crack
Repairing of kiln shell crackmkpq pasha
 
Repairing of kiln shell crack
Repairing of kiln shell crackRepairing of kiln shell crack
Repairing of kiln shell crackmkpq pasha
 

Similar to STUDY OF MICRO STRUCTURE OF HEAT TREADTED EN8 STEEL (20)

Comparison of Mechanical Properties of Austempered, Normalized and As-Weld Ca...
Comparison of Mechanical Properties of Austempered, Normalized and As-Weld Ca...Comparison of Mechanical Properties of Austempered, Normalized and As-Weld Ca...
Comparison of Mechanical Properties of Austempered, Normalized and As-Weld Ca...
 
Analysis and Improvement of Distortion of Lathe Machine Main Spindle
Analysis and Improvement of Distortion of Lathe Machine Main SpindleAnalysis and Improvement of Distortion of Lathe Machine Main Spindle
Analysis and Improvement of Distortion of Lathe Machine Main Spindle
 
Effect of Heat Treatment on Corrosion Behavior of Spring Steels
Effect of Heat Treatment on Corrosion Behavior of Spring SteelsEffect of Heat Treatment on Corrosion Behavior of Spring Steels
Effect of Heat Treatment on Corrosion Behavior of Spring Steels
 
Effect of Subzero Treatment on Microstructure and Material Properties of EN...
Effect of Subzero Treatment on Microstructure and Material  Properties of EN...Effect of Subzero Treatment on Microstructure and Material  Properties of EN...
Effect of Subzero Treatment on Microstructure and Material Properties of EN...
 
Influence of Heat Treatment on Mechanical Properties of Aisi1040 Steel
Influence of Heat Treatment on Mechanical Properties of Aisi1040 SteelInfluence of Heat Treatment on Mechanical Properties of Aisi1040 Steel
Influence of Heat Treatment on Mechanical Properties of Aisi1040 Steel
 
Study and Analysis on Heat Treatment Process and Microstructure of Low Carbon...
Study and Analysis on Heat Treatment Process and Microstructure of Low Carbon...Study and Analysis on Heat Treatment Process and Microstructure of Low Carbon...
Study and Analysis on Heat Treatment Process and Microstructure of Low Carbon...
 
IJERD (www.ijerd.com) International Journal of Engineering Research and Devel...
IJERD (www.ijerd.com) International Journal of Engineering Research and Devel...IJERD (www.ijerd.com) International Journal of Engineering Research and Devel...
IJERD (www.ijerd.com) International Journal of Engineering Research and Devel...
 
IJERD(www.ijerd.com)International Journal of Engineering Research and Develop...
IJERD(www.ijerd.com)International Journal of Engineering Research and Develop...IJERD(www.ijerd.com)International Journal of Engineering Research and Develop...
IJERD(www.ijerd.com)International Journal of Engineering Research and Develop...
 
SuperCoolingFinal Lab
SuperCoolingFinal LabSuperCoolingFinal Lab
SuperCoolingFinal Lab
 
Effect of Subzero Treatment on Microstructure and Material Properties of EN24...
Effect of Subzero Treatment on Microstructure and Material Properties of EN24...Effect of Subzero Treatment on Microstructure and Material Properties of EN24...
Effect of Subzero Treatment on Microstructure and Material Properties of EN24...
 
Effect of Hardness and Wear Resistance on En 353 Steel by Heat Treatment
Effect of Hardness and Wear Resistance on En 353 Steel by Heat  Treatment Effect of Hardness and Wear Resistance on En 353 Steel by Heat  Treatment
Effect of Hardness and Wear Resistance on En 353 Steel by Heat Treatment
 
Study on Influence of heat treatment on Tribological properties of mild steel
Study on Influence of heat treatment on Tribological properties of mild steelStudy on Influence of heat treatment on Tribological properties of mild steel
Study on Influence of heat treatment on Tribological properties of mild steel
 
H0351046052
H0351046052H0351046052
H0351046052
 
Development of laboratory scale salt bath furnace
Development of laboratory scale salt bath furnaceDevelopment of laboratory scale salt bath furnace
Development of laboratory scale salt bath furnace
 
Mechanical property assessment of austempered and conventionally hardened aisi
Mechanical property assessment of austempered and conventionally hardened aisiMechanical property assessment of austempered and conventionally hardened aisi
Mechanical property assessment of austempered and conventionally hardened aisi
 
An assessment of the microstraft
An assessment of the microstraftAn assessment of the microstraft
An assessment of the microstraft
 
New ppt cold working process
New ppt cold working processNew ppt cold working process
New ppt cold working process
 
Steady state thermal analysis of a 4-stroke single
Steady state thermal analysis of a 4-stroke singleSteady state thermal analysis of a 4-stroke single
Steady state thermal analysis of a 4-stroke single
 
Repairing of kiln shell crack
Repairing of kiln shell crackRepairing of kiln shell crack
Repairing of kiln shell crack
 
Repairing of kiln shell crack
Repairing of kiln shell crackRepairing of kiln shell crack
Repairing of kiln shell crack
 

Recently uploaded

Comparative study of High-rise Building Using ETABS,SAP200 and SAFE., SAFE an...
Comparative study of High-rise Building Using ETABS,SAP200 and SAFE., SAFE an...Comparative study of High-rise Building Using ETABS,SAP200 and SAFE., SAFE an...
Comparative study of High-rise Building Using ETABS,SAP200 and SAFE., SAFE an...Erbil Polytechnic University
 
National Level Hackathon Participation Certificate.pdf
National Level Hackathon Participation Certificate.pdfNational Level Hackathon Participation Certificate.pdf
National Level Hackathon Participation Certificate.pdfRajuKanojiya4
 
Energy Awareness training ppt for manufacturing process.pptx
Energy Awareness training ppt for manufacturing process.pptxEnergy Awareness training ppt for manufacturing process.pptx
Energy Awareness training ppt for manufacturing process.pptxsiddharthjain2303
 
welding defects observed during the welding
welding defects observed during the weldingwelding defects observed during the welding
welding defects observed during the weldingMuhammadUzairLiaqat
 
Work Experience-Dalton Park.pptxfvvvvvvv
Work Experience-Dalton Park.pptxfvvvvvvvWork Experience-Dalton Park.pptxfvvvvvvv
Work Experience-Dalton Park.pptxfvvvvvvvLewisJB
 
Autonomous emergency braking system (aeb) ppt.ppt
Autonomous emergency braking system (aeb) ppt.pptAutonomous emergency braking system (aeb) ppt.ppt
Autonomous emergency braking system (aeb) ppt.pptbibisarnayak0
 
Crystal Structure analysis and detailed information pptx
Crystal Structure analysis and detailed information pptxCrystal Structure analysis and detailed information pptx
Crystal Structure analysis and detailed information pptxachiever3003
 
"Exploring the Essential Functions and Design Considerations of Spillways in ...
"Exploring the Essential Functions and Design Considerations of Spillways in ..."Exploring the Essential Functions and Design Considerations of Spillways in ...
"Exploring the Essential Functions and Design Considerations of Spillways in ...Erbil Polytechnic University
 
Mine Environment II Lab_MI10448MI__________.pptx
Mine Environment II Lab_MI10448MI__________.pptxMine Environment II Lab_MI10448MI__________.pptx
Mine Environment II Lab_MI10448MI__________.pptxRomil Mishra
 
THE SENDAI FRAMEWORK FOR DISASTER RISK REDUCTION
THE SENDAI FRAMEWORK FOR DISASTER RISK REDUCTIONTHE SENDAI FRAMEWORK FOR DISASTER RISK REDUCTION
THE SENDAI FRAMEWORK FOR DISASTER RISK REDUCTIONjhunlian
 
Input Output Management in Operating System
Input Output Management in Operating SystemInput Output Management in Operating System
Input Output Management in Operating SystemRashmi Bhat
 
Correctly Loading Incremental Data at Scale
Correctly Loading Incremental Data at ScaleCorrectly Loading Incremental Data at Scale
Correctly Loading Incremental Data at ScaleAlluxio, Inc.
 
Katarzyna Lipka-Sidor - BIM School Course
Katarzyna Lipka-Sidor - BIM School CourseKatarzyna Lipka-Sidor - BIM School Course
Katarzyna Lipka-Sidor - BIM School Coursebim.edu.pl
 
Risk Management in Engineering Construction Project
Risk Management in Engineering Construction ProjectRisk Management in Engineering Construction Project
Risk Management in Engineering Construction ProjectErbil Polytechnic University
 
Engineering Drawing section of solid
Engineering Drawing     section of solidEngineering Drawing     section of solid
Engineering Drawing section of solidnamansinghjarodiya
 
Arduino_CSE ece ppt for working and principal of arduino.ppt
Arduino_CSE ece ppt for working and principal of arduino.pptArduino_CSE ece ppt for working and principal of arduino.ppt
Arduino_CSE ece ppt for working and principal of arduino.pptSAURABHKUMAR892774
 
Virtual memory management in Operating System
Virtual memory management in Operating SystemVirtual memory management in Operating System
Virtual memory management in Operating SystemRashmi Bhat
 
Earthing details of Electrical Substation
Earthing details of Electrical SubstationEarthing details of Electrical Substation
Earthing details of Electrical Substationstephanwindworld
 

Recently uploaded (20)

Comparative study of High-rise Building Using ETABS,SAP200 and SAFE., SAFE an...
Comparative study of High-rise Building Using ETABS,SAP200 and SAFE., SAFE an...Comparative study of High-rise Building Using ETABS,SAP200 and SAFE., SAFE an...
Comparative study of High-rise Building Using ETABS,SAP200 and SAFE., SAFE an...
 
National Level Hackathon Participation Certificate.pdf
National Level Hackathon Participation Certificate.pdfNational Level Hackathon Participation Certificate.pdf
National Level Hackathon Participation Certificate.pdf
 
Energy Awareness training ppt for manufacturing process.pptx
Energy Awareness training ppt for manufacturing process.pptxEnergy Awareness training ppt for manufacturing process.pptx
Energy Awareness training ppt for manufacturing process.pptx
 
welding defects observed during the welding
welding defects observed during the weldingwelding defects observed during the welding
welding defects observed during the welding
 
Work Experience-Dalton Park.pptxfvvvvvvv
Work Experience-Dalton Park.pptxfvvvvvvvWork Experience-Dalton Park.pptxfvvvvvvv
Work Experience-Dalton Park.pptxfvvvvvvv
 
Autonomous emergency braking system (aeb) ppt.ppt
Autonomous emergency braking system (aeb) ppt.pptAutonomous emergency braking system (aeb) ppt.ppt
Autonomous emergency braking system (aeb) ppt.ppt
 
POWER SYSTEMS-1 Complete notes examples
POWER SYSTEMS-1 Complete notes  examplesPOWER SYSTEMS-1 Complete notes  examples
POWER SYSTEMS-1 Complete notes examples
 
Crystal Structure analysis and detailed information pptx
Crystal Structure analysis and detailed information pptxCrystal Structure analysis and detailed information pptx
Crystal Structure analysis and detailed information pptx
 
"Exploring the Essential Functions and Design Considerations of Spillways in ...
"Exploring the Essential Functions and Design Considerations of Spillways in ..."Exploring the Essential Functions and Design Considerations of Spillways in ...
"Exploring the Essential Functions and Design Considerations of Spillways in ...
 
Mine Environment II Lab_MI10448MI__________.pptx
Mine Environment II Lab_MI10448MI__________.pptxMine Environment II Lab_MI10448MI__________.pptx
Mine Environment II Lab_MI10448MI__________.pptx
 
THE SENDAI FRAMEWORK FOR DISASTER RISK REDUCTION
THE SENDAI FRAMEWORK FOR DISASTER RISK REDUCTIONTHE SENDAI FRAMEWORK FOR DISASTER RISK REDUCTION
THE SENDAI FRAMEWORK FOR DISASTER RISK REDUCTION
 
Input Output Management in Operating System
Input Output Management in Operating SystemInput Output Management in Operating System
Input Output Management in Operating System
 
Correctly Loading Incremental Data at Scale
Correctly Loading Incremental Data at ScaleCorrectly Loading Incremental Data at Scale
Correctly Loading Incremental Data at Scale
 
Katarzyna Lipka-Sidor - BIM School Course
Katarzyna Lipka-Sidor - BIM School CourseKatarzyna Lipka-Sidor - BIM School Course
Katarzyna Lipka-Sidor - BIM School Course
 
Risk Management in Engineering Construction Project
Risk Management in Engineering Construction ProjectRisk Management in Engineering Construction Project
Risk Management in Engineering Construction Project
 
Engineering Drawing section of solid
Engineering Drawing     section of solidEngineering Drawing     section of solid
Engineering Drawing section of solid
 
Arduino_CSE ece ppt for working and principal of arduino.ppt
Arduino_CSE ece ppt for working and principal of arduino.pptArduino_CSE ece ppt for working and principal of arduino.ppt
Arduino_CSE ece ppt for working and principal of arduino.ppt
 
Virtual memory management in Operating System
Virtual memory management in Operating SystemVirtual memory management in Operating System
Virtual memory management in Operating System
 
young call girls in Green Park🔝 9953056974 🔝 escort Service
young call girls in Green Park🔝 9953056974 🔝 escort Serviceyoung call girls in Green Park🔝 9953056974 🔝 escort Service
young call girls in Green Park🔝 9953056974 🔝 escort Service
 
Earthing details of Electrical Substation
Earthing details of Electrical SubstationEarthing details of Electrical Substation
Earthing details of Electrical Substation
 

STUDY OF MICRO STRUCTURE OF HEAT TREADTED EN8 STEEL

  • 1. Sakib Ali Saqueeb Ali Anis Haider Md Javed Raja Ansari Muddasir Ali Mondal Sourav Kumar Mahato 130207075 130207079 140307132 140307136 140307137 140307145
  • 2. 1. Abstract 2. Introduction 3. Objective 4. Introduction To En-8 Steel 5. Properties Of En-8 Steel 6. Heat Treatment Process 7. Universal Testing Machine 8. Sample Preparation 9. Optical Microscope 10.Comparison Of Microstructures 11.Inference 12.Reference
  • 3. Steels are generally heat treated in order to achieve desired changes in their microstructure and mechanical properties. The effect of heat treatment cycle on the microstructure and some mechanical properties of EN8 steel have been studied and presented in this presentation. The heat treatment cycles given are Annealing, normalizing, hardening and tempering are the most important heat treatments often used to modify the microstructure and mechanical properties of engineering materials particularly steels. Sample of steel is purchased and various specimens are prepared for tests of mechanical properties, the changes in properties are examined and studied. Finally the heat treated sample was examined in the microscope. In the specimen, grains were differentiated and impurity particle could be seen clearly. The microstructure of the specimen was snapped on 100X, 200X, 500X, and 1000X. Then, analysis and comparison of the microstructure is done.
  • 4.  Heat treatment and microstructure studies have always been a wide area of research for mechanical engineers  We come across steel in our life on an everyday basis. We can find its influence in our life in almost everything we do, we use or we look at. The steel used for this research however is a medium carbon EN-8 steel AISI 1040. It is alloyed and it is used to make things like shafts, keys, stressed pins. The steel with its immense practical applications are an important component in everybody's life.  EN8 is a very popular grade of through-hardening medium carbon steel, which is readily machined able in any condition. EN8 is suitable for the manufacture of parts such as general-purpose axles and shafts, gears, bolts and studs.
  • 5.  To treat the En 8 steel in quenching annealing and normalizing.  To treat the En 8 steel in single tempering after quenching annealing and normalizing .  To measured tensile strength by universal testing machine (UTM) .  To compare the hardness of En8 steel after quenching annealing and normalizing.  To compare the micro-structure of the specimen after different heat treatment process.
  • 6.  EN8 is an alloyed medium carbon steel grade with reasonable tensile strength. It is normally supplied in the cold drawn or as rolled condition. Tensile properties can vary but are usually between 500-800 N/mm². EN8 is widely used for applications which require better properties than mild steel but does not justify the costs of an alloy steel. EN8 can be flame or induction hardened to produce a good surface hardness with moderate wear resistance.
  • 7.  EN8 carbon steel is a common medium carbon and medium tensile steel, with improved strength over mild steel, through-hardening medium carbon steel.  Readily machinable in any condition.  It can be further surface-hardened by induction processes, producing components with enhanced wear resistance.  In its heat treated forms possesses good homogenous metallurgical structures, giving consistent machining properties  Suitable for the manufacture of parts such as general-purpose axles and shafts, gears, bolts and studs.  Good heat treatment results on sections be achievable.
  • 8. Max Stress 700-850N/mm^2 Yield stress 465N/mm^2 min Max Elongation 16% min Impact KCV 28 Joules min Hardness 201-255 Brinell MECHANICAL PROPERTIES
  • 9. En8 specification chemical composition carbon 0.36-0.44% silicon 0.10-0.40% manganese 0.60-1.00% Sulphur 0.050Max phosphorus 0.050Max
  • 10. The sample was received as a round bar. Later on it was cut to desired specified measurement as per our requirement. Later the specimens were undergone through various heat treatment processes.  Heat treatment is a combination of timed heating and cooling applied to a particular metal or alloy in the solid state in such ways as to produce certain microstructure and desired mechanical properties. The heat treatment of steel was done at different temperatures of 950OC, 975OC, 1000OC, 1025OC by using muffle furnace. At each temperature 6 samples were kept to be heated.
  • 11.  A furnace is a device used for high- temperature heating.  A furnace used for many things, such as the extraction of metal from ore or in oil refineries and other chemical plants.  The heat energy to fuel a furnace may be supplied directly by fuel combustion, by electricity such as the electric arc furnace, or through induction heating in induction furnaces.  It serves as a reactor to provide heats to the reaction. The design of the furnaces varies, however the basic features are most common among all of them.
  • 12. Specimen of EN-8 steel rod was first preheated at 15OC per minute to 950OC in a furnace and then held there for 30 minutes such that the temperature homogeneity occurs at all section of the specimens for austentization. After holding for 30 minutes, switch off the furnace and open the furnace door to allow the samples to cool inside the furnace until red heat is gone. Take out the samples and air cool to 65OC in air take out the samples which are at the austenitizing temperature, submerge in oil bath, and water quenched to the room temperature.
  • 13. To remove any preexisting anomalies of material properties, the sample were first subject to a careful annealing cycle: preheating to 950OC, hold for 15 min. slow (stepwise) heating to 950OC; 200-400-600-800-950OC; hold for 15 min at each step. Holding for ½ hrs at 950OC, slow cooling and switch off furnace. Leave samples inside until cooled to 480OC. brisk cooling open furnace door, cool to room temperature.
  • 14. Normalizing process for steels is defined as heating the steel to austenite phase and cooling it in the air. It is carried out by heating the steel approximately 500C above the upper critical temperature followed by cooling in air to room temperature, or at no greater than 1 bar pressure using nitrogen if the process is being run in a vacuum furnace. Normalizing temperatures usually vary from 8100c to 9300C.
  • 15. Temper the EN8 component immediately after quenching whilst tools are still hand warm. Re-heat the EN8 component to the tempering temperature then soak for one hour per 25 millimeter of total thickness (2 hours minimum) Cool in air. For most applications tempering of EN8 will be between 550-660°C.
  • 16. Sl. No. Heat Treated Sample Force (KN) 1. Quenching (Without Tempering) 251 2. Annealing (Without Tempering) 152 3. Normalizing (Without Tempering) 168 4. Quenching (With Tempering) 207 5. Annealing (With Tempering) 118 6. Normalizing (With Tempering) 165 Heat treated samples were tested for various mechanical properties. Average HRC readings were determined by taking several readings at different positions on the samples, using Rockwell hardness tester. For tensile properties, standard tensile specimens were loaded into 400-KN Universal Testing Machine hooked up to a data logger.
  • 17. A machine used to test specimens for tensile strength, compressive strength, shear strength and to perform bend test along other important laboratory tests. The primary use of the testing machine is to create the stress strain diagram. Once the diagram is generated, a pencil and straight edge or computer algorithm can be used to calculate yield strength, Young's Modulus, tensile strength or total elongation.
  • 18. Tool Steel Material Sample Mark Rockwell Hardness C-HRC Rockwell Hardness B-HRB Brinell Hardness HB EN-8 Annealing 12 91 187 Annealing with Tempering 1 82 155 Quenching 42 113 392 Quenching with Tempering 63 - 685 Normalizing 47 115 446 Normalizing with Tempering 22 99 234 Hardness of EN-8 Steel was determined using Brinell and Rockwell
  • 19. Proper preparation of metallographic specimens to determine microstructure and content requires that a rigid step-by-step process be followed. In sequence, the steps included cutting, mounting, course grinding, fine grinding, polishing, etching and microscopic examination. Specimens must be kept clean and preparation procedure carefully followed in order to reveal accurate microstructures. This operation was performed using a power hacksaw. this process is involve cutting a small piece of the work piece by a tool consisting of a series of narrowly spaced teeth, called a saw blade. Sawing is used to separate work parts into two or more pieces, or to cut off an unwanted section of a part.
  • 20. Grinding is the most common form of abrasive machining. It is a material cutting process which engages an abrasive tool whose cutting elements are grains of abrasive material known as grit. These grits are characterized by sharp cutting points, high hot hardness, chemical stability and wear resistance. The grits are held together by a suitable bonding material to give shape of an abrasive tool. Metal Polishing sometimes known as Finishing or Buffing is the process of removing scratches and abrasions from a surface, and creating the desired brightness of finish on that surface. Polishing, like using sand paper, consists of procedures each of which is less abrasive than the previous. A combination of polishing buffing wheels and compounds are used with a buffing machine or a household electric drill (pneumatic tools may also be used but only at relatively low speeds of 4000 rpm max.)
  • 21. The specimen was placed on the table under the fume hood with the polished surface up. 1. The surface was cleaned with alcohol and let dried. 2. A few drops of nital solution (2%) were applied to the specimen surface covering the entire metallic surface of the specimen using the eye dropper. 3. After 20 to 30 seconds. The etchant was rinsed into the sink with the water and it is quickly rinsed with alcohol. 4. The sample was dried again. The sample was examined in the optical microscope. In the specimen, grains were differentiated and impurity particles could be seen clearly. Metallurgical microscope was used to view the specimen at various magnifications and the microstructural aspect of the material was noted. The microstructure of the specimen was snapped on 100X, 200X, 500X, 1000X zooming lenses.
  • 22. The optical microscope, often referred to as light microscope, is a type of microscope which uses visible light and a system of lenses to magnify images of small samples. The image from an optical microscope can be captured by normal light-sensitive cameras to generate a micrograph. Compound optical microscopes are typically used to examine a smear, a squash preparation, or a thinly sectioned slice of some material. A common use of non-transmitted lighting is to study the thin structure of metals and minerals, where the light is reflected from the examined surface. It can produce a magnified image of a specimen up to 1000X and, at high magnifications, are used to study thin specimens as they have a very limited depth of field.
  • 23. The figure depicts microstructure of ‘As received material’ (which is EN-8 steel prior to heat treatment) at 200X zoom, from our objective point of view we consider this microstructure as our reference for further analysis. We can observe from this microstructure the pearlite and ferrite structure clearly. We can also observe non uniformity of the grain size and its coarse nature, the ferrite and pearlite microstructure are also non uniform. The material does not possess good wear resistance.
  • 24. The quenched specimens would have their austenites transformed to martensites. These are fine, needle-like structures which are very strong and hard, but very brittle. The transformation of austenite to martensite by a diffusion less shear type transformation in quenching is also responsible for higher hardness obtained and this property is attributed to the effectiveness of the interstitial carbon in hindering the dislocation motion. After the hardened steel tempered the prevalent martensite is an unstable structure and the carbon atoms diffuse from martensite to form a carbide precipitate and the concurrent formation of ferrite and cementite. Fig. Quenching with tempering Fig. Quenching without tempering
  • 25. If we now observed the microstructure of normalized with tempering steel we can see the coarse grains are produced. The grain size diameter is increased. Because of tempering the heating temp is low and cooling rate is low so nuclei formation will be less. The grain boundary is less than the normalized steel, void also decreases. It increases the dislocation movement because of this ductility of the material will also increase. Fig. Normalizing (200X) Fig. Normalizing with tempering (200X)
  • 26. If we observe the microstructure of annealing with that of annealing along with tempering we can see the fine grains are transformed into coarsened grains due to which void is decreased. The grain size diameter is increased .Because in tempering the heating temp.is low and cooling rate is low so nuclei formation will be less. The grain boundary is less than the annealed steel. As a result of tempering the martensite gets transformed into tempered martensite and thus as a result hardness of the sample decreases. Fig. Annealing (200X) Fig. Annealing With Tempering (200X)
  • 27. The following conclusion has been drawn from the experimental result and discussion is made. The EN8 steel are subjected to different heat treatment sequences: annealing, normalizing, quenching and tempering at different temperatures at 2000C, 4000C, 6000C, 8000C, 9500C. Heat treated specimens were mechanically tested for tensile properties, ductility, and hardness.  After quenching the tensile strength and hardness was increased due the formation of martensitic structure. The crystal grain size was reduced.  After annealing it is observed that the hardness is reduced which softens the specimen, the grain size is refined which in turns improves the machinability of EN8 steel.  After normalizing it is observed that uniform ferrite plus pearlite microstructure is established and uniform grain size obtained.  Tempering the specimen after undergoing above process was found to have many changes like the ductility and toughness was increased with some loss of strength, hardness and ultimate tensile strength, it also possess good corrosion resistance.
  • 28. 1. krishisanskriti.org/Publication.html 2. O.P. Khanna, material science & metallurgy (Dhanpat Rai Publications, 11th Reprint-2007). 3. Elements of Metallurgy and Engineering Alloys. Product code-05224G, F.C. Campbell. www.asminternational.org 4. ASM International 1991, ASM Handbook: Heat Treatment, Vol. 4, American Society for Metals Park, Ohio 5. ASTM E18. 2008, Standard Test Method for Rockwell Hardness of Metallic Materials, American Society of Testing and Materials. 6. D. A. Fadare, T. G. Fadara and O. Y. Akanbi (2011) ―Effect of Heat Treatment on Mechanical. 7. Romesh C Sharma, principles of heat treatment of steels (New Age International Publishers, New Delhi, 2008) 8. International Journal of Engineering Research and Development ISSN: 2278-067X, Volume 2, Issue 1 (July 2012), PP. 07-13 www.ijerd.com 9. Journal of minerals and materials characterization and engineering, 2012, 11, 859-862, published online September 2012 10.Highpeaksteels.com 11.Metals4u.co.uk